SABIC Innovative Plastics ULTEM 2212EPR Polyetherimide (North America)

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)
 Export data to your CAD/FEA program

Subcategory: Polyetherimide; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesMetricEnglishComments
Density1.4 g/cc0.0506 lb/in³ ASTM D 792
Linear Mold Shrinkage0.005 - 0.007 cm/cm0.005 - 0.007 in/in Flow, 0.125 inch; ASTM D 955
Linear Mold Shrinkage, Transverse0.005 - 0.007 cm/cm0.005 - 0.007 in/in 0.125 inch; ASTM D 955
Melt Flow15 g/10 min15 g/10 min 337C/6.6 kgf; ASTM D 1238

Mechanical Properties
Tensile Strength @ Break108 MPa15600 psi Type I, 0.2 in/min; ASTM D 638
Tensile Strength @ Yield108 MPa15600 psi Type I, 0.2 in/min; ASTM D 638
Elongation at Break3 %3 % Type I, 0.2 in/min; ASTM D 638
Elongation at Yield3 %3 % Type I, 0.2 in/min; ASTM D 638
Tensile Modulus5.79 GPa840 ksi 0.2 in/min; ASTM D 638
Flexural Modulus5.1 GPa740 ksi 0.10 in/min, 4" span; ASTM D 790
Flexural Modulus5.52 GPa800 ksi 0.05 in/min, 2" span; ASTM D 790
Flexural Strength172 MPa25000 psi 0.10 in/min, 4" span; ASTM D 790
Flexural Yield Strength172 MPa25000 psi 0.05 in/min, 2" span; ASTM D 790
Izod Impact, Unnotched4.81 J/cm9 ft-lb/in 73F; ASTM D 4812
Gardner Impact @ 23°C12.2 J9 ft-lb Instrumented Impact Total Energy, 73°F; ASTM D 3763
Izod Impact, Notched0.587 J/cm1.1 ft-lb/in 73F; ASTM D 256

Electrical Properties
Arc Resistance120 - 180 sec120 - 180 sec Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495
Comparative Tracking Index100 - 175 V100 - 175 V (+/- 0.125 inch); PLC Code 4; UL 746A
Hot Wire Ignition, HWI60 - 120 sec60 - 120 sec (+/- 0.125 inch); PLC Code 1; UL 746A
High Amp Arc Ignition, HAIMax 15 arcsMax 15 arcs Surface (+/- 0.125 inch); PLC Code 4; UL 746A
High Voltage Arc-Tracking Rate, HVTRMin 150 mm/minMin 5.91 in/min (+/- 0.125 inch); PLC Code 4; UL 746A

Thermal Properties
CTE, linear 68°F36 µm/m-°C20 µin/in-°F Flow, -40F to 100F; ASTM E 831
CTE, linear 68°F, Transverse to Flow72 µm/m-°C40 µin/in-°F from -40F to 100F; ASTM E 831
Deflection Temperature at 0.46 MPa (66 psi)210 °C410 °F 0.125 inch, unannealed; ASTM D 648
Deflection Temperature at 0.46 MPa (66 psi)213 °C415 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)205 °C401 °F 0.125 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)207 °C405 °F 0.250 inch, unannealed; ASTM D 648
Vicat Softening Point210 °C410 °F Rate B; ASTM D 1525
UL RTI, Electrical105 °C221 °F UL 746B
UL RTI, Mechanical with Impact105 °C221 °F UL 746B
UL RTI, Mechanical without Impact105 °C221 °F UL 746B
Flammability, UL94V-0V-0 0.016 in.

Descriptive Properties
UL File Number, USAE121562 
Printer friendly version Printer friendly version


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Instant Quotes for Quick Parts!Upload your 3D CAD model, select process, quantity, material, and instantly receive your unique, binding quote.

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。