SABIC Innovative Plastics ULTEM 2310 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.51 g/cc | 0.0546 lb/in³ | ASTM D 792 |
| Linear Mold Shrinkage | 0.002 - 0.004 cm/cm | 0.002 - 0.004 in/in | Flow, 0.125 inch; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.002 - 0.004 cm/cm | 0.002 - 0.004 in/in | 0.125 inch; ASTM D 955 |
| Melt Flow | 7.6 g/10 min | 7.6 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Break | 159 MPa | 23000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 169 MPa | 24500 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 2 % | 2 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 9.24 GPa | 1340 ksi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 9.24 GPa | 1340 ksi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Strength | 221 MPa | 32000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Izod Impact, Notched | 0.854 J/cm | 1.6 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 4.38 J/cm | 8.2 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Electrical Properties |
|
| Arc Resistance | 60 - 120 sec | 60 - 120 sec | Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495 |
| Comparative Tracking Index | 100 - 175 V | 100 - 175 V | (+/- 0.125 inch); PLC Code 4; UL 746A |
| Hot Wire Ignition, HWI | 60 - 120 sec | 60 - 120 sec | (+/- 0.125 inch); PLC Code 1; UL 746A |
| High Amp Arc Ignition, HAI | Max 15 arcs | Max 15 arcs | Surface (+/- 0.125 inch); PLC Code 4; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 80 - 150 mm/min | 3.15 - 5.91 in/min | (+/- 0.125 inch); PLC Code 3; UL 746A |
Thermal Properties |
|
| CTE, linear, 212°F (100°C) | 41.4 µm/m-°C | 23 µin/in-°F | Cross Flow; 0F to 300F; ASTM E 831 |
| CTE, linear, 212°F (100°C) | 16.2 µm/m-°C | 9 µin/in-°F | Flow, 0F to 300F; ASTM E 831 |
| Deflection Temperature at 1.8 MPa (264 psi) | 210 °C | 410 °F | 0.250 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 180 °C | 356 °F | UL 746B |
| UL RTI, Mechanical with Impact | 170 °C | 338 °F | UL 746B |
| UL RTI, Mechanical without Impact | 180 °C | 356 °F | UL 746B |
| Flammability, UL94 | V-0 | V-0 | 0.01 in. |
| Flammability, UL94 | 7 | 7 | 0.048 in. |
Descriptive Properties | |
| UL File Number, USA | E121562 | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|