SABIC Innovative Plastics ULTEM 8015 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
Physical Properties | Metric | English | Comments |
|
Density | 1.29 g/cc | 0.0466 lb/in³ | ASTM D 792 |
Linear Mold Shrinkage | 0.004 - 0.005 cm/cm | 0.004 - 0.005 in/in | Flow, 0.125 inch; ASTM D 955 |
Linear Mold Shrinkage, Transverse | 0.006 - 0.008 cm/cm | 0.006 - 0.008 in/in | 0.125 inch; ASTM D 955 |
Melt Flow | 2.7 g/10 min | 2.7 g/10 min | 295C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
Tensile Strength @ Break | 89.6 MPa | 13000 psi | Type I, 0.2 in/min; ASTM D 638 |
Tensile Strength @ Yield | 96.5 MPa | 14000 psi | Type I, 0.2 in/min; ASTM D 638 |
Elongation at Break | 80 % | 80 % | Type I, 0.2 in/min; ASTM D 638 |
Tensile Modulus | 3.31 GPa | 480 ksi | 0.2 in/min; ASTM D 638 |
Flexural Modulus | 3.17 GPa | 460 ksi | 0.10 in/min, 4" span; ASTM D 790 |
Flexural Yield Strength | 145 MPa | 21000 psi | 0.10 in/min, 4" span; ASTM D 790 |
Gardner Impact @ 23°C | 56.5 J | 41.7 ft-lb | Instrumented Impact Energy @ peak, -22°F; ASTM D 3763 |
Gardner Impact @ 23°C | 71.7 J | 52.9 ft-lb | Instrumented Impact Energy @ peak, 73°F; ASTM D 3763 |
Izod Impact, Notched | 0.641 J/cm | 1.2 ft-lb/in | 73F; ASTM D 256 |
Izod Impact, Notched | 20.8 J/cm | 39 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Thermal Properties |
|
Deflection Temperature at 1.8 MPa (264 psi) | 188 °C | 370 °F | 0.250 inch, unannealed; ASTM D 648 |
Flammability Test | 45 | 45 | OSU 2 minute heat, release rate; KW-Min/m2; FAR 25.853 |
Flammability Test | 5 | 5 | Vertical Burn, length; inches; FAR 25.853 |
Flammability Test | 80 | 80 | OSU Peak Heat Release Rate (horizontal); KW/m2; FAR 25.853 |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|