SABIC Innovative Plastics VALOX 4521 PBT (North America)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.53 g/cc | 0.0553 lb/in³ | ASTM D 792 |
Mechanical Properties |
|
| Tensile Strength @ Break | 91 MPa | 13200 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 89.6 MPa | 13000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 2.5 % | 2.5 % | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Yield | 2.4 % | 2.4 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 3.52 GPa | 510 ksi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 4.96 GPa | 720 ksi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Strength | 138 MPa | 20000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Unnotched | 4.81 J/cm | 9 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched | 0.427 J/cm | 0.8 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Arc Resistance | 120 - 180 sec | 120 - 180 sec | Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495 |
| Comparative Tracking Index | 250 - 400 V | 250 - 400 V | (+/- 0.125 inch); PLC Code 2; UL 746A |
| Hot Wire Ignition, HWI | Min 120 sec | Min 120 sec | (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Amp Arc Ignition, HAI | Min 120 arcs | Min 120 arcs | Surface (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | Min 150 mm/min | Min 5.91 in/min | (+/- 0.125 inch); PLC Code 4; UL 746A |
Thermal Properties |
|
| Deflection Temperature at 0.46 MPa (66 psi) | 219 °C | 426 °F | 0.125 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 205 °C | 401 °F | 0.125 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 130 °C | 266 °F | UL 746B |
| UL RTI, Mechanical with Impact | 130 °C | 266 °F | UL 746B |
| UL RTI, Mechanical without Impact | 130 °C | 266 °F | UL 746B |
| Flammability, UL94 | V-0 | V-0 | 0.03 in. |
Descriptive Properties | |
| UL File Number, GLOBAL | E161759 | |
| UL File Number, USA | E121562 | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|