| Physical Properties | Metric | English | Comments |
|
| Density | 1.43 g/cc | 0.0517 lb/in³ | ASTM D 792 |
| Density | 1.43 g/cc | 0.0517 lb/in³ | ISO 1183 |
| Moisture Absorption at Equilibrium | 0.2 % | 0.2 % | (23 C / 50% RH) 1L; ISO 15512 |
| Water Absorption at Saturation | 1 % | 1 % | 23C; ISO 62 |
| Linear Mold Shrinkage | 0.003 - 0.005 cm/cm | 0.003 - 0.005 in/in | Flow; ASTM D 955 |
| Melt Flow | 5 g/10 min | 5 g/10 min | cm3/10min; Melt Volume Rate, MVR at 360C/5.0 kg; ISO 1133 |
Mechanical Properties |
|
| Hardness, H358/30 | 145 MPa | 21000 psi | ISO 2039/1 |
| Tensile Strength, Ultimate | 135 MPa | 19600 psi | 5 mm/min; ISO 527 |
| Elongation at Break | 3 % | 3 % | 5 mm/min; ISO 527 |
| Tensile Modulus | 7.2 GPa | 1040 ksi | 1 mm/min; ISO 527 |
| Flexural Modulus | 5.8 GPa | 841 ksi | 2 mm/min; ISO 178 |
| Flexural Strength | 180 MPa | 26100 psi | 2 mm/min; ISO 178 |
| Izod Impact, Unnotched (ISO) | 40 kJ/m² | 19 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1U |
| Izod Impact, Unnotched Low Temp (ISO) | 40 kJ/m² | 19 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1U |
Electrical Properties |
|
| Volume Resistivity | 1e+015 ohm-cm | 1e+015 ohm-cm | IEC 60093 |
| Surface Resistivity per Square | Min 1e+015 ohm | Min 1e+015 ohm | ROA; IEC 60093 |
| Dielectric Constant | 3 | 3 | 1 MHz; IEC 60250 |
| Dielectric Constant | 3.2 | 3.2 | 50 Hz; IEC 60250 |
| Dielectric Strength | 16 kV/mm | 406 kV/in | in oil, 3.2 mm; IEC 60243-1 |
| Dielectric Strength | 26 kV/mm | 660 kV/in | in oil, 1.6 mm; IEC 60243-1 |
| Dissipation Factor | 0.0016 | 0.0016 | 50 Hz; IEC 60250 |
| Dissipation Factor | 0.0043 | 0.0043 | 1 MHz; IEC 60250 |
| Comparative Tracking Index | 100 V | 100 V | M; IEC 60112/3rd |
| Comparative Tracking Index | 150 V | 150 V | IEC 60112/3rd |
| Comparative Tracking Index | 150 V | 150 V | Stand. Black; IEC 60112/3rd |
Thermal Properties |
|
| CTE, linear 100°C | 20 µm/m-°C | 11.1 µin/in-°F | 23C-150C, flow; ISO 11359-2 |
| CTE, linear 100°C | 50 µm/m-°C | 27.8 µin/in-°F | 23C-150C, cross flow; ISO 11359-2 |
| Deflection Temperature at 0.46 MPa (66 psi) | 210 °C | 410 °F | HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be |
| Deflection Temperature at 1.8 MPa (264 psi) | 205 °C | 401 °F | HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae |
| Vicat Softening Point | 220 °C | 428 °F | B/50; ISO 306 |
| Vicat Softening Point | 222 °C | 432 °F | B/120; ISO 306 |
| Vicat Softening Point | 225 °C | 437 °F | A/50; ISO 306 |
| UL RTI, Electrical | 105 °C | 221 °F | UL 746B |
| UL RTI, Mechanical with Impact | 105 °C | 221 °F | UL 746B |
| UL RTI, Mechanical without Impact | 105 °C | 221 °F | UL 746B |
| Flammability, UL94 | V-0 | V-0 | 1.5 mm |
| Flammability, UL94 | 7 | 7 | 94-1.5 mm |
| Flammability Test | 1 | 1 | mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2 |
| Oxygen Index | 47 % | 47 % | ISO 4589 |
| Glow Wire Test | 960 °C | 1760 °F | Passes at 3.2 mm; EDF HN60S02 |
| Glow Wire Test | 960 °C | 1760 °F | Passes at 3.2 mm; IEC 60695-2-1 |
Descriptive Properties |
|
| Ball Pressure Test, 125 C +/- 2 C | PASSES | IEC 60035-1 |
|