SABIC Innovative Plastics ULTEM 2212 Polyetherimide (Europe)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their European product line. This product is also a part of their North American product line.
Physical Properties | Metric | English | Comments |
|
Density | 1.43 g/cc | 0.0517 lb/in³ | ASTM D 792 |
Density | 1.43 g/cc | 0.0517 lb/in³ | ISO 1183 |
Linear Mold Shrinkage | 0.003 - 0.005 cm/cm | 0.003 - 0.005 in/in | Flow; ASTM D 955 |
Mechanical Properties |
|
Tensile Strength, Ultimate | 75 MPa | 10900 psi | 5 mm/min; ISO 527 |
Elongation at Break | 8 % | 8 % | 5 mm/min; ISO 527 |
Tensile Modulus | 4.5 GPa | 653 ksi | 1 mm/min; ISO 527 |
Flexural Yield Strength | 135 MPa | 19600 psi | 2 mm/min; ISO 178 |
Compressive Modulus | 4.5 GPa | 653 ksi | ASTM D 695 |
Izod Impact, Unnotched (ISO) | 30 kJ/m² | 14.3 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1U |
Thermal Properties |
|
Thermal Conductivity | 0.28 W/m-K | 1.94 BTU-in/hr-ft²-°F | ISO 8302 |
Deflection Temperature at 0.46 MPa (66 psi) | 202 °C | 396 °F | HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be |
Deflection Temperature at 1.8 MPa (264 psi) | 189 °C | 372 °F | HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae |
Vicat Softening Point | 211 °C | 412 °F | B/120; ISO 306 |
Vicat Softening Point | 220 °C | 428 °F | Rate B; ASTM D 1525 |
UL RTI, Electrical | 170 °C | 338 °F | UL 746B |
UL RTI, Mechanical with Impact | 170 °C | 338 °F | UL 746B |
UL RTI, Mechanical without Impact | 170 °C | 338 °F | UL 746B |
Flammability, UL94 | V-0 | V-0 | 0.41 mm |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|