SABIC Innovative Plastics ULTEM 6200 Polyetherimide (Europe)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their European product line.
Physical Properties | Metric | English | Comments |
|
Density | 1.43 g/cc | 0.0517 lb/in³ | ASTM D 792 |
Water Absorption | 0.22 % | 0.22 % | 24 hours; ASTM D 570 |
Mechanical Properties |
|
Tensile Strength, Ultimate | 145 MPa | 21000 psi | ASTM D 638 |
Elongation at Break | 4 % | 4 % | ASTM D 638 |
Tensile Modulus | 6.9 GPa | 1000 ksi | DIN 53457 |
Flexural Modulus | 6.5 GPa | 943 ksi | DIN 53457 |
Flexural Strength | 210 MPa | 30500 psi | DIN 53452 |
Ultimate Compressive Strength | 170 MPa | 24700 psi | ASTM D 695 |
Shear Strength | 95 MPa | 13800 psi | ASTM D 732 |
Izod Impact, Notched | 0.8 J/cm | 1.5 ft-lb/in | 23 C; ASTM D 256 |
Izod Impact, Unnotched | 4 J/cm | 7.49 ft-lb/in | 23 C; ASTM D 4812 |
Electrical Properties |
|
Volume Resistivity | 1e+015 ohm-cm | 1e+015 ohm-cm | IEC 60093 |
Dielectric Strength | 23 kV/mm | 584 kV/in | in oil, 1.6 mm; IEC 60243-1 |
Thermal Properties |
|
Deflection Temperature at 0.46 MPa (66 psi) | 225 °C | 437 °F | ASTM D 648 |
Deflection Temperature at 1.8 MPa (264 psi) | 223 °C | 433 °F | ASTM D 648 |
Vicat Softening Point | 243 °C | 469 °F | Rate B; ASTM D 1525 |
Flammability, UL94 | V-0 | V-0 | 1.5 mm |
Flammability Test | 3.2 | 3.2 | mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2 |
NBS Smoke Density | 4 | 4 | Flaming, Ds 4 min; ASTM E 662 |
Oxygen Index | 44 % | 44 % | ISO 4589 |
Descriptive Properties | |
Needle Flame Test, 3.2 mm, Burn Time s | PASSES | IEC 60695-2-2 |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use