Physical Properties | Metric | English | Comments |
|
Density | 1.45 g/cc | 0.0524 lb/in³ | ASTM D 792 |
Density | 1.45 g/cc | 0.0524 lb/in³ | ISO 1183 |
Moisture Absorption at Equilibrium | 0.03 % | 0.03 % | (23 C / 50% RH) 1L; ISO 15512 |
Water Absorption at Saturation | 0.15 % | 0.15 % | 23C; ISO 62 |
Linear Mold Shrinkage | 0.003 - 0.007 cm/cm | 0.003 - 0.007 in/in | Flow; ASTM D 955 |
Linear Mold Shrinkage, Transverse | 0.004 - 0.01 cm/cm | 0.004 - 0.01 in/in | ASTM D 955 |
Melt Flow | 16 g/10 min | 16 g/10 min | cm3/10min; Melt Volume Rate, MVR at 250C/2.16 kg; ISO 1133 |
Mechanical Properties |
|
Hardness, H358/30 | 120 MPa | 17400 psi | ISO 2039/1 |
Tensile Strength, Ultimate | 110 MPa | 16000 psi | 5 mm/min; ISO 527 |
Elongation at Break | 3 % | 3 % | 5 mm/min; ISO 527 |
Tensile Modulus | 7 GPa | 1020 ksi | 1 mm/min; ISO 527 |
Flexural Modulus | 6 GPa | 870 ksi | 2 mm/min; ISO 178 |
Flexural Strength | 140 MPa | 20300 psi | 2 mm/min; ISO 178 |
Izod Impact, Notched (ISO) | 7 kJ/m² | 3.33 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1A |
Izod Impact, Unnotched (ISO) | 45 kJ/m² | 21.4 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1U |
Izod Impact, Unnotched Low Temp (ISO) | 35 kJ/m² | 16.7 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1U |
Izod Impact, Notched, Low Temp (ISO) | 6 kJ/m² | 2.86 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1A |
Charpy Impact Unnotched | 4 J/cm² | 19 ft-lb/in² | 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 0.5 J/cm² | 2.38 ft-lb/in² | at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | 3 J/cm² | 14.3 ft-lb/in² | at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
Charpy Impact, Notched | 0.6 J/cm² | 2.86 ft-lb/in² | 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Electrical Properties |
|
Volume Resistivity | Min 1e+015 ohm-cm | Min 1e+015 ohm-cm | IEC 60093 |
Surface Resistivity per Square | Min 1e+015 ohm | Min 1e+015 ohm | ROA; IEC 60093 |
Dielectric Constant | 3 | 3 | 1 MHz; IEC 60250 |
Dielectric Constant | 3.2 | 3.2 | 50 Hz; IEC 60250 |
Dielectric Strength | 16 kV/mm | 406 kV/in | in oil, 3.2 mm; IEC 60243-1 |
Dielectric Strength | 24 kV/mm | 610 kV/in | in oil, 1.6 mm; IEC 60243-1 |
Dielectric Strength | 26 kV/mm | 660 kV/in | in oil, 0.8 mm; IEC 60243-1 |
Dissipation Factor | 0.001 | 0.001 | 50 Hz; IEC 60250 |
Dissipation Factor | 0.014 | 0.014 | 1 MHz; IEC 60250 |
Comparative Tracking Index | 250 V | 250 V | IEC 60112/3rd |
Comparative Tracking Index | 300 V | 300 V | Stand. Black; IEC 60112/3rd |
Comparative Tracking Index | 325 V | 325 V | Electr Grey; IEC 60112/3rd |
Thermal Properties |
|
CTE, linear 20°C | 40 µm/m-°C | 22.2 µin/in-°F | 23C-80C, flow; ISO 11359-2 |
CTE, linear 20°C Transverse to Flow | 80 µm/m-°C | 44.4 µin/in-°F | 23C-80C; ISO 11359-2 |
CTE, linear 100°C | 80 µm/m-°C | 44.4 µin/in-°F | 23C-150C, cross flow; ISO 11359-2 |
Deflection Temperature at 0.46 MPa (66 psi) | 220 °C | 428 °F | HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be |
Deflection Temperature at 1.8 MPa (264 psi) | 205 °C | 401 °F | HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae |
Vicat Softening Point | 210 °C | 410 °F | B/50; ISO 306 |
Vicat Softening Point | 215 °C | 419 °F | B/120; ISO 306 |
Flammability, UL94 | HB | HB | 0.84 mm; UL 94 by GE |
Flammability, UL94 | HB | HB | 0.84 mm |
Glow Wire Test | 750 °C | 1380 °F | Passes at 1 mm; EDF HN60S02 |
Glow Wire Test | 750 °C | 1380 °F | Passes at 1 mm; IEC 60695-2-1 |
Descriptive Properties |
|
Ball Pressure Test, 125 C +/- 2 C | PASSES | IEC 60035-1 |
|