Physical Properties | Metric | English | Comments |
|
Density | 1.5 g/cc | 0.0542 lb/in³ | ASTM D 792 |
Density | 1.5 g/cc | 0.0542 lb/in³ | ISO 1183 |
Water Absorption | 0.06 % | 0.06 % | 24 hours; ASTM D 570 |
Moisture Absorption at Equilibrium | 0.06 % | 0.06 % | (23 C / 50% RH) 1L; ISO 15512 |
Water Absorption at Saturation | 0.09 % | 0.09 % | 23C; ISO 62 |
Linear Mold Shrinkage | 0.004 - 0.006 cm/cm | 0.004 - 0.006 in/in | Flow; ASTM D 955 |
Linear Mold Shrinkage, Transverse | 0.005 - 0.009 cm/cm | 0.005 - 0.009 in/in | ASTM D 955 |
Melt Flow | 8 g/10 min | 8 g/10 min | cm3/10min; Melt Volume Rate, MVR at 250C/2.16 kg; ISO 1133 |
Mechanical Properties |
|
Hardness, Rockwell R | 119 | 119 | ISO 2039/2 |
Hardness, H358/30 | 122 MPa | 17700 psi | ISO 2039/1 |
Tensile Strength, Ultimate | 110 MPa | 16000 psi | ASTM D 638 |
Tensile Strength, Ultimate | 120 MPa | 17400 psi | 5 mm/min; ISO 527 |
Elongation at Break | 2 % | 2 % | 5 mm/min; ISO 527 |
Elongation at Break | 3 % | 3 % | ASTM D 638 |
Tensile Modulus | 8.9 GPa | 1290 ksi | 1 mm/min; ISO 527 |
Flexural Modulus | 6.9 GPa | 1000 ksi | DIN 53457 |
Flexural Modulus | 8 GPa | 1160 ksi | 2 mm/min; ISO 178 |
Flexural Strength | 170 MPa | 24700 psi | DIN 53452 |
Flexural Strength | 170 MPa | 24700 psi | 2 mm/min; ISO 178 |
Ultimate Compressive Strength | 115 MPa | 16700 psi | ASTM D 695 |
Shear Strength | 56 MPa | 8120 psi | ASTM D 732 |
Izod Impact, Notched | 1.05 J/cm | 1.97 ft-lb/in | 23 C; ASTM D 256 |
Izod Impact, Notched (ISO) | 8 kJ/m² | 3.81 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1A |
Izod Impact, Unnotched (ISO) | 50 kJ/m² | 23.8 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1U |
Izod Impact, Unnotched Low Temp (ISO) | 50 kJ/m² | 23.8 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1U |
Izod Impact, Notched, Low Temp (ISO) | 7 kJ/m² | 3.33 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1A |
Charpy Impact Unnotched | 4.5 J/cm² | 21.4 ft-lb/in² | 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 0.65 J/cm² | 3.09 ft-lb/in² | at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | 5 J/cm² | 23.8 ft-lb/in² | at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
Charpy Impact, Notched | 0.75 J/cm² | 3.57 ft-lb/in² | 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Electrical Properties |
|
Volume Resistivity | Min 1e+015 ohm-cm | Min 1e+015 ohm-cm | IEC 60093 |
Surface Resistivity per Square | Min 1e+015 ohm | Min 1e+015 ohm | ROA; IEC 60093 |
Dielectric Constant | 3.2 | 3.2 | 1 MHz; IEC 60250 |
Dielectric Constant | 3.3 | 3.3 | 50 Hz; IEC 60250 |
Dielectric Constant | 3.6 | 3.6 | 100 Hz; IEC 60250 |
Dielectric Strength | 16 kV/mm | 406 kV/in | in oil, 3.2 mm; IEC 60243-1 |
Dielectric Strength | 23 kV/mm | 584 kV/in | in oil, 1.6 mm; IEC 60243-1 |
Dielectric Strength | 24 kV/mm | 610 kV/in | Short time, 3.2 mm; ASTM D 149 |
Dielectric Strength | 24 kV/mm | 610 kV/in | Short time, 1.0 mm; IEC 60243-1 |
Dielectric Strength | 30 kV/mm | 762 kV/in | in oil, 0.8 mm; IEC 60243-1 |
Dissipation Factor | 0.001 | 0.001 | 50 Hz; IEC 60250 |
Dissipation Factor | 0.0014 | 0.0014 | 100 Hz; IEC 60250 |
Dissipation Factor | 0.013 | 0.013 | 1 MHz; IEC 60250 |
Arc Resistance | 62 sec | 62 sec | Tungsten; ASTM D 495 |
Comparative Tracking Index | 150 V | 150 V | M; IEC 60112/3rd |
Comparative Tracking Index | 250 V | 250 V | IEC 60112/3rd |
Comparative Tracking Index | 250 V | 250 V | Stand. Black; IEC 60112/3rd |
Comparative Tracking Index | 275 V | 275 V | Electr Grey; IEC 60112/3rd |
Hot Wire Ignition, HWI | 66 sec | 66 sec | UL 746A |
High Amp Arc Ignition, HAI | 15 arcs | 15 arcs | on surface; UL 746A |
High Voltage Arc-Tracking Rate, HVTR | 1.8 mm/min | 0.0709 in/min | UL 746A |
Thermal Properties |
|
CTE, linear 20°C | 25 µm/m-°C | 13.9 µin/in-°F | 23C-80C, flow; ISO 11359-2 |
CTE, linear 20°C Transverse to Flow | 100 µm/m-°C | 55.6 µin/in-°F | 23C-80C; ISO 11359-2 |
CTE, linear 100°C | 105 µm/m-°C | 58.3 µin/in-°F | 23C-150C, cross flow; ISO 11359-2 |
Deflection Temperature at 0.46 MPa (66 psi) | 210 °C | 410 °F | HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be |
Deflection Temperature at 0.46 MPa (66 psi) | 215 °C | 419 °F | ASTM D 648 |
Deflection Temperature at 1.8 MPa (264 psi) | 150 °C | 302 °F | HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae |
Deflection Temperature at 1.8 MPa (264 psi) | 175 °C | 347 °F | ASTM D 648 |
Vicat Softening Point | 180 °C | 356 °F | B/50; ISO 306 |
Vicat Softening Point | 180 °C | 356 °F | B/120; ISO 306 |
Vicat Softening Point | 215 °C | 419 °F | Rate B; ASTM D 1525 |
Vicat Softening Point | 217 °C | 423 °F | A/50; ISO 306 |
UL RTI, Electrical | 125 °C | 257 °F | UL 746B |
UL RTI, Mechanical with Impact | 110 °C | 230 °F | UL 746B |
UL RTI, Mechanical without Impact | 125 °C | 257 °F | UL 746B |
Flammability, UL94 | HB | HB | 1.5 mm |
Glow Wire Test | 750 °C | 1380 °F | Passes at 1 mm; EDF HN60S02 |
Glow Wire Test | 750 °C | 1380 °F | Passes at 1 mm; IEC 60695-2-1 |
Descriptive Properties |
|
Ball Pressure Test, 125 C +/- 2 C | PASSES | IEC 60035-1 |
|
Printer friendly version |