SABIC Innovative Plastics VALOX 830X PBT (Europe)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their European product line.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.54 g/cc | 0.0556 lb/in³ | ASTM D 792 |
| Density | 1.54 g/cc | 0.0556 lb/in³ | ISO 1183 |
| Moisture Absorption at Equilibrium | 0.08 % | 0.08 % | (23 C / 50% RH) 1L; ISO 15512 |
| Water Absorption at Saturation | 0.2 % | 0.2 % | 23C; ISO 62 |
| Linear Mold Shrinkage | 0.004 - 0.009 cm/cm | 0.004 - 0.009 in/in | Flow; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.006 - 0.011 cm/cm | 0.006 - 0.011 in/in | ASTM D 955 |
| Melt Flow | 8 g/10 min | 8 g/10 min | cm3/10min; Melt Volume Rate, MVR at 265C/1.2 kg; ISO 1133 |
Mechanical Properties |
|
| Tensile Strength, Ultimate | 105 MPa | 15200 psi | 5 mm/min; ISO 527 |
| Elongation at Break | 3 % | 3 % | 5 mm/min; ISO 527 |
| Tensile Modulus | 8 GPa | 1160 ksi | 1 mm/min; ISO 527 |
| Flexural Modulus | 7 GPa | 1020 ksi | 2 mm/min; ISO 178 |
| Flexural Yield Strength | 150 MPa | 21800 psi | 2 mm/min; ISO 178 |
| Izod Impact, Notched (ISO) | 5 kJ/m² | 2.38 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1A |
| Izod Impact, Unnotched (ISO) | 40 kJ/m² | 19 ft-lb/in² | 80*10*4 +23 C; ISO 180/ 1U |
| Izod Impact, Unnotched Low Temp (ISO) | 30 kJ/m² | 14.3 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1U |
| Izod Impact, Notched, Low Temp (ISO) | 5 kJ/m² | 2.38 ft-lb/in² | 80*10*4 -30 C; ISO 180/ 1A |
| Charpy Impact Unnotched | 3.5 J/cm² | 16.7 ft-lb/in² | 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
| Charpy Impact, Notched, Low Temp | 0.4 J/cm² | 1.9 ft-lb/in² | at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
| Charpy Impact, Unnotched Low Temp | 2.5 J/cm² | 11.9 ft-lb/in² | at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
| Charpy Impact, Notched | 0.5 J/cm² | 2.38 ft-lb/in² | 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Thermal Properties |
|
| Vicat Softening Point | 175 °C | 347 °F | B/120; ISO 306 |
| Flammability, UL94 | HB | HB | 1.5 mm |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|