SABIC Innovative Plastics ULTEM® 2300N Polyetherimide, 30% Glass Filled, Injection Grade
Subcategory: Filled/Reinforced Thermoplastic; Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Data for 3.2 mm (1/8 in) samples unless otherwise noted. Data provided by GE Plastics.
Physical Properties | Metric | English | Comments |
|
Density | 1.51 g/cc | 0.0546 lb/in³ | ASTM D792 |
Water Absorption | 0.16 % | 0.16 % | 24 hrs; 20°C; ASTM D570 |
Linear Mold Shrinkage | 0.002 - 0.004 cm/cm | 0.002 - 0.004 in/in | 3.2 mm sample |
Melt Flow | 4.2 g/10 min | 4.2 g/10 min | 335°C/6.6kg; ASTM D1238 |
Mechanical Properties |
|
Tensile Strength, Ultimate | 169 MPa | 24500 psi | ASTM D638 |
Elongation at Break | 3 % | 3 % | ASTM D638 |
Flexural Modulus | 9 GPa | 1310 ksi | 3.2 mm sample; ASTM D790 |
Izod Impact, Notched | 0.9 J/cm | 1.69 ft-lb/in | 3.2 mm sample; ASTM D256 |
Electrical Properties |
|
Electrical Resistivity | 3e+016 ohm-cm | 3e+016 ohm-cm | ASTM D257 |
Thermal Properties |
|
Deflection Temperature at 0.46 MPa (66 psi) | 212 °C | 414 °F | 6.4 mm sample; ASTM D648 |
Deflection Temperature at 1.8 MPa (264 psi) | 210 °C | 410 °F | 6.4 mm (0.25 in.) sample; ASTM D648 |
Vicat Softening Point | 227 °C | 441 °F | 5 kg; ASTM D1525 |
Processing Properties |
|
Processing Temperature | 348 - 398 °C | 658 - 748 °F | Suggested injection molding melt temperature |
Mold Temperature | 135 - 162 °C | 275 - 324 °F | |
Drying Temperature | 149 °C | 300 °F | |
Dry Time | 4 - 6 hour | 4 - 6 hour | 24 hr Max. |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|