MatWeb - Material Property Data 用 MatWeb 登广告!    Register Now
越过59,000 以上, 金属、塑料、陶瓷和合成物的数据资料库。
MatWeb - Material Property Data 主页  •  搜寻  •  工具  •  供应商  •  文件夹  •  有关我们  •  常用问题  •  登录   •  English English English 
  搜寻方法:  高级先进 | 材料类型 | 特性 | 构成份  | 商标  | 制造商
    Search

COMSOL CD

EMS-Grivory Grilon® A 28 Nylon 6, Dry As Molded

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)
 Export data to your CAD/FEA program

Subcategory: Nylon; Nylon 6; Polymer; Thermoplastic

Material Notes:
Grilon A 28 is an unreinforced, standard PA6 injection molding grade with normal melt viscosity.

Grilon A 28 has wide variety of applications in all market sectors, automotive, electrical, leisure and sport, e. g. clips, covers, housings.

Information provided by EMS-Grivory

Physical PropertiesMetricEnglishComments
Density1.14 g/cc0.0412 lb/in³ ISO 1183
Water Absorption3 %3 % 23°C / 50% RH; ISO 62
Water Absorption at Saturation9 %9 % ISO 62
Linear Mold Shrinkage0.008 cm/cm0.008 in/in ISO 294
Linear Mold Shrinkage, Transverse0.0095 cm/cm0.0095 in/in ISO 294

Mechanical Properties
Hardness, Shore D140140 ISO 868
Tensile Strength at Break70 MPa10200 psi 50 mm/min; ISO 527
Elongation at Break5 %5 % 50 mm/min; ISO 527
Tensile Modulus3.3 GPa479 ksi 1 mm/min; ISO 527
Charpy Impact UnnotchedMin 10 J/cm²Min 47.6 ft-lb/in² ISO 179/1eU
Charpy Impact, Notched, Low Temp0.4 J/cm²1.9 ft-lb/in²  -30°C; ISO 179/1eA
Charpy Impact, Unnotched Low TempMin 10 J/cm²Min 47.6 ft-lb/in²  -30°C; ISO 179/1eU
Charpy Impact, Notched0.4 J/cm²1.9 ft-lb/in² ISO 179/1eA

Electrical Properties
Volume Resistivity1e+014 ohm-cm1e+014 ohm-cm IEC 60093
Dielectric Strength30 kV/mm762 kV/in IEC 60243-1

Thermal Properties
CTE, linear 20°C100 µm/m-°C55.6 µin/in-°F trans. (23-55°C); ISO 11359
CTE, linear 20°C70 µm/m-°C38.9 µin/in-°F long. (23-55°C); ISO 11359
Melting Point222 °C432 °F ISO 11357
Maximum Service Temperature, Air70 - 90 °C158 - 194 °F Long Term; ISO 2578
Maximum Service Temperature, Air160 °C320 °F Short Term; ISO 2578
Deflection Temperature at 0.46 MPa (66 psi)170 °C338 °F ISO 75
Deflection Temperature at 1.8 MPa (264 psi)55 °C131 °F ISO 75
Flammability, UL94HBHB 0.8 mm; ISO 1210

Processing Properties
Processing Temperature80 °C176 °F Tool
Rear Barrel Temperature260 °C500 °F Zone 3
Middle Barrel Temperature255 °C491 °F Zone 2
Front Barrel Temperature250 °C482 °F Zone 1
Nozzle Temperature260 °C500 °F 
Melt Temperature240 - 300 °C464 - 572 °F Basic machine settings
Drying TemperatureMax 100 °CMax 212 °F Vacuum Oven
Drying TemperatureMax 80 °CMax 176 °F Desiccant Dryer (dew point at -25°F)
Dry Time4 - 12 hour4 - 12 hour Vacuum Oven
Dry Time4 - 12 hour4 - 12 hour Desiccant Dryer (dew point at -25°F)
Hold Pressure30 - 80 MPa4350 - 11600 psi 
Back Pressure0.5 - 1.5 MPa72.5 - 218 psi 
Screw Speed50 - 100 rpm50 - 100 rpm 
Printer friendly version Printer friendly version


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Instant Quotes for Quick Parts!Upload your 3D CAD model, select process, quantity, material, and instantly receive your unique, binding quote.

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。