EMS-Grivory Grilon® FE 8023 Natural Nylon 6, Dry As Molded
Subcategory: Nylon; Nylon 6; Polymer; Thermoplastic
Material Notes: Grilon FE 8023 natural is a new heat stabilized injection molding grade based on Polyamide 6.Information provided by EMS-Grivory
Physical Properties | Metric | English | Comments |
|
Density | 1.15 g/cc | 0.0415 lb/in³ | ISO 1183 |
Linear Mold Shrinkage | 0.009 cm/cm | 0.009 in/in | ISO 294 |
Linear Mold Shrinkage, Transverse | 0.006 cm/cm | 0.006 in/in | ISO 294 |
Melt Flow | 57.5 g/10 min | 57.5 g/10 min | 275°C / 5kg; ISO 11133 |
Mechanical Properties |
|
Tensile Strength at Break | 100 MPa | 14500 psi | 5 mm/min; ISO 527 |
Elongation at Break | 3 % | 3 % | 5 mm/min; ISO 527 |
Tensile Modulus | 4.6 GPa | 667 ksi | 1 mm/min; ISO 527 |
Charpy Impact Unnotched | 7 J/cm² | 33.3 ft-lb/in² | ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 0.4 J/cm² | 1.9 ft-lb/in² | -30°C; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | 6.5 J/cm² | 30.9 ft-lb/in² | -30°C; ISO 179/1eU |
Charpy Impact, Notched | 0.4 J/cm² | 1.9 ft-lb/in² | ISO 179/1eA |
Thermal Properties |
|
Melting Point | 220 °C | 428 °F | ISO 11357 |
Deflection Temperature at 0.46 MPa (66 psi) | 180 °C | 356 °F | ISO 75 |
Deflection Temperature at 1.8 MPa (264 psi) | 100 °C | 212 °F | ISO 75 |
Processing Properties |
|
Melt Temperature | 240 - 300 °C | 464 - 572 °F | Injection molding |
Mold Temperature | 80 - 100 °C | 176 - 212 °F | Injection molding |
Hold Pressure | 50 - 75 MPa | 7250 - 10900 psi | |
Back Pressure | 0.5 - 1.5 MPa | 72.5 - 218 psi | |
Screw Speed | 50 - 100 rpm | 50 - 100 rpm | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|