PolyOne Geon® 90401 Vinyl Alloy - Flexible (FPVC alloy)
Subcategory: Polymer; Thermoplastic; Vinyl
Material Notes:
Description/Features: Applications: Market: Processing Method: Disclaimer: Note: Automotive OEM approval(s). Information provided by PolyOne Corporation.
Physical Properties | Metric | English | Comments |
|
Specific Gravity | 1.24 g/cc | 0.0448 lb/in³ | ASTM D792 |
Mechanical Properties |
|
Hardness, Shore A | 75 | 75 | 15 sec; ASTM D2240 |
Tensile Strength, Ultimate | 14.2 MPa | 2060 psi | Type 4 - Flexibles, 20 in/min; ASTM D638 |
Elongation at Break | 313 % | 313 % | Type 4 - Flexibles, 20 in/min; ASTM D638 |
Tear Strength | 36.1 kN/m | 206 pli | Die C (graves), 20 in/min; ASTM D624 |
Thermal Properties |
|
Flammability Test | 0 | 0 | in/min; FMVSS 302 |
Optical Properties |
|
Gloss | 3.5 % | 3.5 % | 60º Gardner; ASTM D523 |
Descriptive Properties | |
Automotive Approval | General Motors, GMP.PVC.077 | |
Cold Flexibility | Pass | -20°F (-29°C), 25 mm, 4 hrs, 0.075 in; GM9503P |
Fogging | 86 % | 3 hrs, 212°F (100°C), 70°F (21°C), after 1 hour; SAE J1756 |
Product Form | Pellets | |
Xenon Weatherometer - Interior | Pass | 1,240 kJ/m², All Colors, dE*; SAE J1885 |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|