Degussa AG Vestamid® DX9321 Black 20% Glass Reinforced Nylon 612 (Dry as Molded)
Subcategory: Filled/Reinforced Thermoplastic; Nylon; Nylon 612; Polymer; Thermoplastic
Key Words: PA612-HI, MH, 14-050, GF20
Material Notes: Description: impact-resistant,20% glass fiber reinforced, heat-stabilized Applications: housings, coverings Information provided by degussa.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.19 g/cc | 0.043 lb/in³ | ISO 1183 |
| Moisture Absorption at Equilibrium | 0.8 % | 0.8 % | 23°C/50% R.H.; ISO 62 |
| Water Absorption at Saturation | 2 % | 2 % | ISO 62 |
| Linear Mold Shrinkage | 0.0066 cm/cm | 0.0066 in/in | 127x12.7x3.2 mm (processing cond. acc. To DIN EN ISO 1874-2) |
| Linear Mold Shrinkage, Transverse | 0.0088 cm/cm | 0.0088 in/in | 127x12.7x3.2 mm (processing cond. acc. To DIN EN ISO 1874-2) |
Mechanical Properties |
|
| Tensile Strength at Break | 109 MPa | 15800 psi | ISO 527-2/1A |
| Elongation at Break | 6 % | 6 % | ISO 527-2/1A |
| Tensile Modulus | 5.45 GPa | 790 ksi | ISO 527-2/1A |
| Charpy Impact Unnotched | 9.3 J/cm² | 44.3 ft-lb/in² | 23°C; ISO 179/1eU |
| Charpy Impact, Notched, Low Temp | 1.1 J/cm² | 5.24 ft-lb/in² | -30°C; ISO 179/1eA |
| Charpy Impact, Unnotched Low Temp | 10.6 J/cm² | 50.4 ft-lb/in² | -30°C; ISO 179/1eU |
| Charpy Impact, Notched | 1.8 J/cm² | 8.57 ft-lb/in² | 23°C; ISO 179/1eA |
Electrical Properties |
|
| Volume Resistivity | 1e+014 ohm-cm | 1e+014 ohm-cm | IEC 60093 |
| Dielectric Constant | 3.1 | 3.1 | 23°C/1 MHz; IEC 60250 |
| Dielectric Constant, Low Frequency | 4.4 | 4.4 | 23°C/100 Hz; IEC 60250 |
| Dissipation Factor | 0.047 | 0.047 | 23°C/1 MHz; IEC 60250 |
| Dissipation Factor, Low Frequency | 0.05 | 0.05 | 23°C/100 Hz; IEC 60250 |
| Comparative Tracking Index | Min 600 V | Min 600 V | Test Solution A, 50 drops; IEC 60112 |
| Comparative Tracking Index | 600 V | 600 V | Test Solution A, 100 drops; IEC 60112 |
Thermal Properties |
|
| CTE, linear 20°C | 50 µm/m-°C | 27.8 µin/in-°F | 23-55°C, Longitudinal; ISO 11359 |
| CTE, linear 20°C | 70 µm/m-°C | 38.9 µin/in-°F | 23-55°C, Transverse; ISO 11359 |
| Melting Point | 215 °C | 419 °F | Peak Temperature; ISO 11357 |
| Deflection Temperature at 0.46 MPa (66 psi) | 208 °C | 406 °F | ISO 75 |
| Deflection Temperature at 1.8 MPa (264 psi) | 189 °C | 372 °F | ISO 75 |
| Vicat Softening Point | 207 °C | 405 °F | 50N; ISO 306 |
| Flammability, UL94 | HB | HB | 1.6 mm |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|