LNP (SABIC Innovative Plastics) VALOX® SMV5871 Polybutylene Terephthalate, 20% Mineral Filler
Subcategory: Filled/Reinforced Thermoplastic; Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Will be VM720. - Features: Low Warpage, Good Dimensional Stability, High Strength
- Forms: Pellets
- Processing Method: Injection Molding
Information provided by LNP, a GE Plastics Company.
| Physical Properties | Metric | English | Comments |
|
| Specific Gravity | 1.48 g/cc | 0.0535 lb/in³ | ASTM D792 |
| Linear Mold Shrinkage | 0.013 - 0.015 cm/cm | 0.013 - 0.015 in/in | 3.18 mm; ASTM D955 |
| Linear Mold Shrinkage, Transverse | 0.012 - 0.014 cm/cm | 0.012 - 0.014 in/in | 3.18 mm; ASTM D955 |
Mechanical Properties |
|
| Tensile Strength at Break | 55.2 MPa | 8010 psi | Type I, 5 mm/min; ASTM D638 |
| Elongation at Break | 2.4 % | 2.4 % | Type I, 5 mm/min; ASTM D638 |
| Tensile Modulus | 4.83 GPa | 701 ksi | 5 mm/min; ASTM D638 |
| Flexural Modulus | 4.65 GPa | 674 ksi | (50.8 mm Span) 1mm/min; ASTM D790 |
| Flexural Strength | 100 MPa | 14500 psi | at Break, (50.8 mm Span) 1mm/min; ASTM D790 |
| Izod Impact, Notched | 0.267 J/cm | 0.5 ft-lb/in | ASTM D256 |
| Izod Impact, Notched | 1.9 J/cm | 3.56 ft-lb/in | Reverse; ASTM D256 |
| Izod Impact, Unnotched | 3.1 J/cm | 5.81 ft-lb/in | ASTM D256 |
| Falling Dart Impact | 5.08 J | 3.75 ft-lb | ASTM D3763 |
Thermal Properties |
|
| CTE, linear 20°C | 47 µm/m-°C | 26.1 µin/in-°F | -40 to 38°C; ASTM D696 |
| CTE, linear 20°C | 61 µm/m-°C | 33.9 µin/in-°F | 60 to 138°C; ASTM D696 |
| CTE, linear 20°C Transverse to Flow | 50 µm/m-°C | 27.8 µin/in-°F | -40 to 38°C; ASTM D696 |
| CTE, linear 20°C Transverse to Flow | 88 µm/m-°C | 48.9 µin/in-°F | 60 to 138°C; ASTM D696 |
| Deflection Temperature at 0.46 MPa (66 psi) | 193 °C | 379 °F | Unannealed (3.18 mm); ASTM D648 |
| Deflection Temperature at 0.46 MPa (66 psi) | 202 °C | 396 °F | Unannealed (6.35 mm); ASTM D648 |
Processing Properties |
|
| Rear Barrel Temperature | 243 - 254 °C | 469 - 489 °F | |
| Middle Barrel Temperature | 249 - 260 °C | 480 - 500 °F | |
| Front Barrel Temperature | 254 - 266 °C | 489 - 511 °F | |
| Nozzle Temperature | 254 - 271 °C | 489 - 520 °F | |
| Melt Temperature | 254 - 277 °C | 489 - 531 °F | |
| Mold Temperature | 65.6 - 93.3 °C | 150 - 200 °F | |
| Drying Temperature | 121 °C | 250 °F | |
| Dry Time | 3 - 12 hour | 3 - 12 hour | |
| Moisture Content | 0.02 % | 0.02 % | Suggested |
| Back Pressure | 0.345 - 0.689 MPa | 50 - 99.9 psi | |
| Clamp Pressure | 41 - 83 MPa | 5950 - 12000 psi | |
| Shot Size | 40 - 80 % | 40 - 80 % | Suggested |
| Vent Depth | 0.0025 - 0.0038 cm | 0.000984 - 0.0015 in | |
| Screw Speed | 50 - 80 rpm | 50 - 80 rpm | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|