Physical Properties | Metric | English | Comments |
|
Specific Gravity | 1.47 g/cc | 0.0531 lb/in³ | ASTM D792 |
Water Absorption | 0.41 % | 0.41 % | 24 hrs; 23°C; ASTM D570 |
Linear Mold Shrinkage | 0.003 cm/cm | 0.003 in/in | 1/8 in (3.2 mm); ASTM D955 |
Mechanical Properties |
|
Hardness, Rockwell R | 122 | 122 | ASTM D785 |
Tensile Strength @ Break | 128 MPa | 18500 psi | ASTM D638 |
Elongation at Break | 3 - 4 % | 3 - 4 % | ASTM D638 |
Tensile Modulus | 5.86 GPa | 850 ksi | ASTM D638 |
Flexural Modulus | 5.52 GPa | 800 ksi | ASTM D638 |
Flexural Yield Strength | 186 MPa | 27000 psi | ASTM D790 |
Compressive Yield Strength | 131 MPa | 19000 psi | ASTM D695 |
Izod Impact, Unnotched | 6.94 J/cm | 13 ft-lb/in | 1/8 in (3.2 mm); ASTM D4812 |
Izod Impact, Notched | 0.641 J/cm | 1.2 ft-lb/in | 1/8 in (3.2 mm); ASTM D256 |
Electrical Properties |
|
Volume Resistivity | Min 1e+012 ohm-cm | Min 1e+012 ohm-cm | ASTM D257 |
Dielectric Constant | 3.9 | 3.9 | 1 MHz; Dry; ASTM D150 |
Dielectric Strength | 15 kV/mm | 380 V/mil | S/T; in oil; ASTM D149 |
Dissipation Factor | 0.007 | 0.007 | 1 MHz; Dry; ASTM D150 |
Thermal Properties |
|
CTE, linear 68°F | 36 µm/m-°C | 20 µin/in-°F | Flow Direction; ASTM E831 |
Thermal Conductivity | 0.288 W/m-K | 2 BTU-in/hr-ft²-°F | Through Plane; ASTM E1530 |
Deflection Temperature at 0.46 MPa (66 psi) | 216 °C | 420 °F | ASTM D648 |
Deflection Temperature at 1.8 MPa (264 psi) | 210 °C | 410 °F | ASTM D648 |
Flammability, UL94 | V-0 | V-0 | 1/16 in (1.5 mm) |
Processing Properties |
|
Melt Temperature | 343 - 377 °C | 650 - 710 °F | |
Mold Temperature | 135 - 177 °C | 275 - 350 °F | |
Drying Temperature | 149 °C | 300 °F | 6 hrs |
Moisture Content | 0.04 % | 0.04 % | |
Dew Point | -31.7 °C | -25 °F | |
Injection Pressure | 68.9 - 103 MPa | 10000 - 15000 psi | |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|
|
|
|
请读关于材料数据的和我们的。询问或评论有关 MatWeb? 请与 联系。我们感谢您对 MatWeb的参与。
本站点由 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。
|
|
|