BASF Elastollan® 1180A10 Wire & Cable Grade Polyurethane Elastomer
Subcategory: Elastomer, TPE; Polymer; Polyurethane, TP; Thermoplastic
Key Words: TPU Rubbers
Material Notes: As with all TPU products this grade must be dried prior to processing. Information provided by BASF Corporation.
Click here to view available vendors for this material.
| Physical Properties | Metric | English | Comments |
|
| Density | 1.11 g/cc | 0.0401 lb/in³ | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D792 |
Mechanical Properties |
|
| Hardness, Shore A | 80 | 80 | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D2240 |
| Tensile Strength, Ultimate | 48 MPa | 6960 psi | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C; ASTM D412 |
| Tensile Strength, Yield | 12 MPa | 1740 psi | Tensile stress at 300% elongation; 0.76 mm (0.030 in) extruded sheet; ASTM D-412 |
| Tensile Strength, Yield | 4.8 MPa | 696 psi | Tensile stress at 100% elongation.; ASTM D-412 |
| Elongation at Break | 625 % | 625 % | on 0.030 in extruded sheet; ASTM D-412 |
| Flexural Modulus | 0.03 GPa | 4.35 ksi | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D790 |
| Tear Strength | 42 kN/m | 240 pli | Split tear strength (ASTM D-1938) on 0.76 mm ( 0.030 inch) extruded sheet |
| Graves Tear Strength | 77 kN/m | 439 pli | on 0.76 mm ( 0.030 inch) extruded sheet; ASTM D624 |
| Taber Abrasion, mg/1000 Cycles | 20 | 20 | H-18 wheel; ASTM D-1044; 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C. |
| Compression Set | 25 % | 25 % | 22 hr at 23°C per ASTM D-395; 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C. |
| Compression Set, Elevated Temperature | 45 % | 45 % | 22 hr @ 70°C; ASTM D-395; 0.080 in molded plaque after curing 20 hrs at 100°C. |
| Tensile Set | 32 % | 32 % | at 200% elongation per ASTM D-412 is on 0.030 in extruded sheet. |
Thermal Properties |
|
| Vicat Softening Point | 90 °C | 194 °F | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D1525 |
| Glass Temperature | -43 °C | -45.4 °F | Pellet sample |
| Flammability, UL94 | HB | HB | Color: NC. 0.83 mm. |
|
Printer friendly version |
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|