SABIC Innovative Plastics LEXAN FL913 Polycarbonate (North America)
Subcategory: Polycarbonate; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
Physical Properties | Original Value | Comments |
|
Density | 1.12 g/cc | Molded Foam; ASTM D 792 |
Density | 1.25 g/cc | ASTM D 792 |
Water Absorption | 0.16 % | 24 hours @ 73F; ASTM D 570 |
Water Absorption at Saturation | 0.32 % | Equilibrium, 73F; ASTM D 570 |
Linear Mold Shrinkage | 0.004 - 0.006 cm/cm | Flow, 0.250 inch; ASTM D 955 |
Mechanical Properties |
|
Tensile Strength @ Yield | 7600 psi | 0.250"; ASTM D 638 |
Elongation at Break | 4.8 % | 0.250"; ASTM D 638 |
Tensile Modulus | 460000 psi | 0.250"; ASTM D 638 |
Flexural Modulus | 510000 psi | 0.250"; ASTM D 790 |
Flexural Yield Strength | 13000 psi | 0.250"; ASTM D 790 |
Izod Impact, Unnotched | 16 ft-lb/in | 73F; ASTM D 4812 |
Thermal Properties |
|
CTE, linear 68°F | 18 µin/in-°F | Flow, -40F to 200F; ASTM E 831 |
Specific Heat Capacity | 0.286 BTU/lb-°F | ASTM C 351 |
Thermal Conductivity | 0.13 W/m-K | ASTM C 177 |
Deflection Temperature at 0.46 MPa (66 psi) | 285 °F | 0.250 inch, unannealed; ASTM D 648 |
Deflection Temperature at 1.8 MPa (264 psi) | 272 °F | 0.250 inch, unannealed; ASTM D 648 |
UL RTI, Electrical | 80 °C | UL 746B |
UL RTI, Mechanical with Impact | 80 °C | UL 746B |
UL RTI, Mechanical without Impact | 80 °C | UL 746B |
Flammability, UL94 | V-0 | 0.152 in. |
Flammability, UL94 | 7 | 0.152 in. |
Flammability Test | 0.97 | FOAM - Flame Class Minimum Density; g/cm3 |
Descriptive Properties | |
Foam Weight Reduction | 10% | Mechanical Properties Reported Herein (0.250") |
Foam Weight Reduction | 10% | Impact Properties Reported Herein (0.250") |
Foam Weight Reduction | 10% | Thermal Properties Reported Herein (0.250") |
Foam Weight Reduction | 10% | Physical Properties Reported Herein (0.250") |
UL File Number, USA | E121562 | |
UV-light, water exposure/immersion | F1 | UL746C |
|
Printer friendly version |
|