Physical Properties | Original Value | Comments |
|
Density | 1.42 g/cc | ASTM D 792 |
Density | 1.42 g/cc | ISO 1183 |
Water Absorption | 0.1 % | 24 hours; ASTM D 570 |
Moisture Absorption at Equilibrium | 0.11 % | (23 C / 50% RH) 1L; ISO 15512 |
Water Absorption at Saturation | 0.26 % | 23C; ISO 62 |
Water Absorption at Saturation | 0.5 % | 100 C; ASTM D 570 |
Linear Mold Shrinkage | 0.002 - 0.004 cm/cm | Flow; ASTM D 955 |
Melt Flow | 10 g/10 min | cm3/10min; Melt Volume Rate, MVR at 265C/10.0 kg; ISO 1133 |
Melt Flow | 4 g/10 min | cm3/10min; Melt Volume Rate, MVR at 300C/1.2 kg; ISO 1133 |
Mechanical Properties |
|
Hardness, Rockwell L | 104 | ISO 2039/2 |
Hardness, H358/30 | 135 MPa | ISO 2039/1 |
Tensile Strength, Ultimate | 75 MPa | 5 mm/min; ISO 527 |
Elongation at Break | 2 % | 5 mm/min; ISO 527 |
Tensile Modulus | 4.5 GPa | 1 mm/min; ISO 527 |
Flexural Modulus | 4.5 GPa | 2 mm/min; ISO 178 |
Flexural Strength | 120 MPa | 2 mm/min; ISO 178 |
Izod Impact, Notched | 0.8 J/cm | 23 C; ASTM D 256 |
Izod Impact, Notched (ISO) | 8 kJ/m² | 80*10*4 +23 C; ISO 180/ 1A |
Izod Impact, Unnotched (ISO) | 40 kJ/m² | 80*10*4 +23 C; ISO 180/ 1U |
Izod Impact, Unnotched Low Temp (ISO) | 40 kJ/m² | 80*10*4 -30 C; ISO 180/ 1U |
Izod Impact, Notched, Low Temp | 0.6 J/cm | at -40 C; ASTM D 256 |
Izod Impact, Notched, Low Temp | 0.7 J/cm | at -20 C; ASTM D 256 |
Izod Impact, Notched, Low Temp | 0.75 J/cm | at 0 C; ASTM D 256 |
Izod Impact, Notched, Low Temp (ISO) | 8 kJ/m² | 80*10*4 -30 C; ISO 180/ 1A |
Charpy Impact Unnotched | 5 J/cm² | 23 C; ISO 179/2C |
Charpy Impact, Notched, Low Temp | 0.6 J/cm² | at -20 C; ISO 179/2C |
Charpy Impact, Notched, Low Temp | 0.7 J/cm² | at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Charpy Impact, Notched | 0.7 J/cm² | 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Charpy Impact, Notched | 0.7 J/cm² | 23 C; ISO 179/2C |
Taber Abrasion, mg/1000 Cycles | 24 | CS-17, 1 kg; GE Test |
Electrical Properties |
|
Volume Resistivity | Min 1e+015 ohm-cm | IEC 60093 |
Surface Resistivity per Square | Min 1e+015 ohm | ROA; IEC 60093 |
Dielectric Constant | 3 | 1 MHz; IEC 60250 |
Dielectric Constant | 3.1 | 50 Hz; IEC 60250 |
Dielectric Strength | 16 kV/mm | in oil, 3.2 mm; IEC 60243-1 |
Dielectric Strength | 20 kV/mm | Short time, 3.2 mm; ASTM D 149 |
Dissipation Factor | 0.001 | 50 Hz; IEC 60250 |
Dissipation Factor | 0.01 | 1 MHz; IEC 60250 |
Arc Resistance | 120 sec | Tungsten; ASTM D 495 |
Comparative Tracking Index | 150 V | IEC 60112/3rd |
Thermal Properties |
|
CTE, linear 20°C | 28 µm/m-°C | 23C-80C, flow; ISO 11359-2 |
Thermal Conductivity | 0.22 W/m-K | ISO 8302 |
Deflection Temperature at 0.46 MPa (66 psi) | 145 °C | HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be |
Deflection Temperature at 0.46 MPa (66 psi) | 153 °C | ASTM D 648 |
Deflection Temperature at 1.8 MPa (264 psi) | 140 °C | HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae |
Deflection Temperature at 1.8 MPa (264 psi) | 148 °C | ASTM D 648 |
Vicat Softening Point | 147 °C | B/50; ISO 306 |
Vicat Softening Point | 150 °C | B/120; ISO 306 |
Vicat Softening Point | 153 °C | A/50; ISO 306 |
Vicat Softening Point | 163 °C | Rate B; ASTM D 1525 |
Vicat Softening Point | 163 °C | VST/A/120; DIN 53460 |
UL RTI, Electrical | 80 °C | UL 746B |
UL RTI, Mechanical with Impact | 80 °C | UL 746B |
UL RTI, Mechanical without Impact | 80 °C | UL 746B |
Flammability, UL94 | V-0 | 1.5 mm |
Flammability Test | 3.2 | mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2 |
Oxygen Index | 33 % | ISO 4589 |
Glow Wire Test | 850 °C | Passes at 1 mm; IEC 60695-2-1 |
Glow Wire Test | 960 °C | Passes at 3.2 mm; IEC 60695-2-1 |
Descriptive Properties |
|
Ball Pressure Test, 125 C +/- 2 C | PASSES | IEC 60035-1 |
Hot Mandrel Test, 300 C | PASSES | CEE10/IIed |
Needle Flame Test, 3.2 mm, Burn Time s | PASSES | IEC 60695-2-2 |
Water Absorption, 24 hours, mg | 10 | DIN 53495 |
|