Aluminum 6061-T6; 6061-T651
Subcategory: 6000 Series Aluminum Alloy; Aluminum Alloy; Metal; Nonferrous Metal
Close Analogs: Composition Notes: Aluminum content reported is calculated as remainder. Composition information provided by the Aluminum Association and is not for design.
Key Words: al6061, UNS A96061; ISO AlMg1SiCu; Aluminium 6061-T6, AD-33 (Russia); AA6061-T6; 6061T6, UNS A96061; ISO AlMg1SiCu; Aluminium 6061-T651, AD-33 (Russia); AA6061-T651
| Component | Wt. % |  | | | Al | 95.8 - 98.6 | | | Cr | 0.04 - 0.35 | | | Cu | 0.15 - 0.4 | | | Fe | Max 0.7 | |
| | Component | Wt. % |  | | | Mg | 0.8 - 1.2 | | | Mn | Max 0.15 | | | Other, each | Max 0.05 | | | Other, total | Max 0.15 | |
| | Component | Wt. % |  | | | Si | 0.4 - 0.8 | | | Ti | Max 0.15 | | | Zn | Max 0.25 | |
|
Material Notes: Information provided by Alcoa, Starmet and the references. General 6061 characteristics and uses: Excellent joining characteristics, good acceptance of applied coatings. Combines relatively high strength, good workability, and high resistance to corrosion; widely available. The T8 and T9 tempers offer better chipping characteristics over the T6 temper. Applications: Aircraft fittings, camera lens mounts, couplings, marines fittings and hardware, electrical fittings and connectors, decorative or misc. hardware, hinge pins, magneto parts, brake pistons, hydraulic pistons, appliance fittings, valves and valve parts; bike frames. Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.
Click here to view available vendors for this material.
| Physical Properties | Metric | English | Comments |
|
| Density | 2.7 g/cc | 0.0975 lb/in³ | AA; Typical |
Mechanical Properties |
|
| Hardness, Brinell | 95 | 95 | AA; Typical; 500 g load; 10 mm ball |
| Hardness, Knoop | 120 | 120 | Converted from Brinell Hardness Value |
| Hardness, Rockwell A | 40 | 40 | Converted from Brinell Hardness Value |
| Hardness, Rockwell B | 60 | 60 | Converted from Brinell Hardness Value |
| Hardness, Vickers | 107 | 107 | Converted from Brinell Hardness Value |
| Ultimate Tensile Strength | 310 MPa | 45000 psi | AA; Typical |
| Tensile Yield Strength | 276 MPa | 40000 psi | AA; Typical |
| Elongation at Break | 12 % | 12 % | AA; Typical; 1/16 in. (1.6 mm) Thickness |
| Elongation at Break | 17 % | 17 % | AA; Typical; 1/2 in. (12.7 mm) Diameter |
| Modulus of Elasticity | 68.9 GPa | 10000 ksi | AA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus. |
| Notched Tensile Strength | 324 MPa | 47000 psi | 2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17. |
| Ultimate Bearing Strength | 607 MPa | 88000 psi | Edge distance/pin diameter = 2.0 |
| Bearing Yield Strength | 386 MPa | 56000 psi | Edge distance/pin diameter = 2.0 |
| Poisson's Ratio | 0.33 | 0.33 | Estimated from trends in similar Al alloys. |
| Fatigue Strength | 96.5 MPa | 14000 psi | AA; 500,000,000 cycles completely reversed stress; RR Moore machine/specimen |
| Fracture Toughness | 29 MPa-m½ | 26.4 ksi-in½ | KIC; TL orientation. |
| Machinability | 50 % | 50 % | 0-100 Scale of Aluminum Alloys |
| Shear Modulus | 26 GPa | 3770 ksi | Estimated from similar Al alloys. |
| Shear Strength | 207 MPa | 30000 psi | AA; Typical |
Electrical Properties |
|
| Electrical Resistivity | 3.99e-006 ohm-cm | 3.99e-006 ohm-cm | AA; Typical at 68°F |
Thermal Properties |
|
| CTE, linear 68°F | 23.6 µm/m-°C | 13.1 µin/in-°F | AA; Typical; Average over 68-212°F range. |
| CTE, linear 250°C | 25.2 µm/m-°C | 14 µin/in-°F | Estimated from trends in similar Al alloys. 20-300°C. |
| Specific Heat Capacity | 0.896 J/g-°C | 0.214 BTU/lb-°F | |
| Thermal Conductivity | 167 W/m-K | 1160 BTU-in/hr-ft²-°F | AA; Typical at 77°F |
| Melting Point | 582 - 652 °C | 1080 - 1205 °F | AA; Typical range based on typical composition for wrought products 1/4 inch thickness or greater; Eutectic melting can be completely eliminated by homogenization. |
| Solidus | 582 °C | 1080 °F | AA; Typical |
| Liquidus | 652 °C | 1205 °F | AA; Typical |
Processing Properties |
|
| Solution Temperature | 529 °C | 985 °F | |
| Aging Temperature | 160 °C | 320 °F | Rolled or drawn products; hold at temperature for 18 hr |
| Aging Temperature | 177 °C | 350 °F | Extrusions or forgings; hold at temperature for 8 hr |
|
Printer friendly version |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|