Uninhibited Leaded Muntz Metal, UNS C36500
Subcategory: Copper Alloy; Metal; Nonferrous Metal
Key Words: 60/40 brass, CDA 365, CZ137, ISO, CuZn39Pb0.5, CEN CW610N, UNS C36800, UNS C36600, UNS C36700, UNS C36800, uninhibited, arsenical, antimonial, phosphorized leaded muntz metal, low leaded brass
| Component | Wt. % |  | | | Cu | 58 - 61 | | | Fe | Max 0.15 | | | Other | Max 0.1 | | | Pb | 0.4 - 0.9 | | | Sn | Max 0.25 | | | Zn | 39.4 | |
|
Material Notes: Fair to excellent corrosion resistance. Excellent machinability. Combines good machinability with excellent hot formability. Applications: main tube sheets for condensers and heat exchangers, support sheets, baffles. Commercial forms available flat products. Rod 61.0% Cu minimum.
| Physical Properties | Original Value | Comments |
|
| Density | 8.41 g/cc | UNS C36500 |
Mechanical Properties |
|
| Hardness, Rockwell F | 80 | M20 temper |
| Tensile Strength, Ultimate | 370 MPa | M20 temper |
| Tensile Strength, Yield | 140 MPa | M20 temper |
| Elongation at Break | 45 % | in 50 mm, M20 temper |
| Modulus of Elasticity | 105 GPa | |
| Poisson's Ratio | 0.35 | Calculated |
| Machinability | 60 % | UNS C36000 (free-cutting brass) = 100% |
| Shear Modulus | 39 GPa | |
Electrical Properties |
|
| Electrical Resistivity | 6.2e-006 ohm-cm | at 20°C (68°F) |
Thermal Properties |
|
| CTE, linear 250°C | 20.8 µm/m-°C | from 20-300°C (68-570°F) |
| Specific Heat Capacity | 0.38 J/g-°C | |
| Thermal Conductivity | 123 W/m-K | at 20°C (68°F) |
| Melting Point | 885 - 900 °C | |
| Solidus | 885 °C | |
| Liquidus | 900 °C | |
Processing Properties |
|
| Annealing Temperature | 425 - 600 °C | |
| Hot-Working Temperature | 625 - 800 °C | |
|
Printer friendly version |