AISI Type 420 Stainless Steel, tested at 205°C (400°F)
Subcategory: Ferrous Metal; Heat Resisting; Metal; Stainless Steel; T 400 Series Stainless Steel
Key Words: UNS S42000, AMS 5506, AMS 5621, ASTM A276, ASTM A314, ASTM A473, ASTM A580, FED QQ-S-763, FED QQ-S-766, FED QQ-W-423, MIL SPEC MIL-S-862, SAE J405 (51420), B.S. 420 S 37, B.S. CDS-18 (U.K), martensitic, DIN 1.4021, AFNOR Z 20 C 13 (Fr), UNI X 20 Cr 13, JIS SUS 420 J1, SS14 2303 (Sweden), ISO 683/13 4
| Component | Wt. % |  | | | C | Min 0.15 | | | Cr | 13 | | | Fe | 85 | | | Mn | Max 1 | | | P | Max 0.04 | | | S | Max 0.03 | | | Si | Max 1 | |
|
Material Notes: 16.0 mm diameter bar, austenitized at 980°C for 30 minutes, oil quench, temper for 2 hours at 28°C above test temperature
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
| Physical Properties | Original Value | Comments |
|
| Density | 7.8 g/cc | |
Mechanical Properties |
|
| Hardness, Brinell | 506 | Converted from Rockwell C Hardness |
| Hardness, Knoop | 562 | Converted from Rockwell C Hardness |
| Hardness, Rockwell C | 51.5 | before testing, 51 after |
| Hardness, Vickers | 541 | Converted from Rockwell C Hardness |
| Tensile Strength, Ultimate | 1820 MPa | |
| Tensile Strength, Yield | 1085 MPa | at 0.2% offset |
| Elongation at Break | 11.5 % | in 50 mm |
| Charpy Impact | 100 J | annealed (tested at room temperature), 14 J quenched and tempered (tested at room temperature) |
| Shear Modulus | 80.7 GPa | |
Electrical Properties |
|
| Electrical Resistivity | 5.5e-005 ohm-cm | at 20°C |
Thermal Properties |
|
| CTE, linear 20°C | 10.3 µm/m-°C | from 0-100°C (32-212°F) |
| CTE, linear 250°C | 10.8 µm/m-°C | at 0-315°C (32-600°F) |
| CTE, linear 500°C | 11.7 µm/m-°C | 0-540°C, 12.2 at 0-650°C |
| Specific Heat Capacity | 0.46 J/g-°C | from 0-100°C (32-212°F) |
| Thermal Conductivity | 24.9 W/m-K | at 100°C |
| Melting Point | 1455 - 1510 °C | |
| Solidus | 1455 °C | |
| Liquidus | 1510 °C | |
| Maximum Service Temperature, Air | 620 °C | Continuous Service |
| Maximum Service Temperature, Air | 735 °C | Intermittent Service |
|
Printer friendly version |
References for this datasheet.

|