Arkema Rilsan® AMN G8 TLD Nylon 12, Graphite Filled (Conditioned)
Subcategory: Filled/Reinforced Thermoplastic; Nylon; Nylon 12; Polymer; Thermoplastic
Close Analogs: Arkema, formed in 2004, was formerly Atofina Chemicals and before that Elf Atochem.
Key Words: PA12; Polyamide 12
Material Notes: Designation ISO 1874-PA12,MHLS,14-010,CD05 Rigid grade with graphite filler for injection molding. Available colors: steel gray. Light and heat stabilized. Mold-release agent. Low friction coefficient. No need of lubricant. Good mechanical properties. Easy filling of the mold due to its well adapted viscosity. Low shrinkage: include 1% on average for the design of the mold. Very good dimensional stability (low moisture absorption). Higher rate of production. Example applications: Moving mechanical parts. ISO data provided by the manufacturer, Arkema.
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
Physical Properties | Original Value | Comments |
|
Density | 1.02 g/cc | |
Melt Flow | 61.5 g/10 min | 235°C/2.16 kg load |
Mechanical Properties |
|
Tensile Strength, Yield | 39 MPa | 50 mm/min |
Elongation at Break | Min 50 % | Nominal Strain; 50 mm/min |
Elongation at Yield | 12 % | 50 mm/min |
Tensile Modulus | 1.36 GPa | 1 mm/min |
Charpy Impact Unnotched | NB | |
Charpy Impact, Notched, Low Temp | 0.42 J/cm² | at -30°C |
Charpy Impact, Unnotched Low Temp | NB | |
Charpy Impact, Notched | 0.44 J/cm² | |
Electrical Properties |
|
Electrical Resistivity | 1e+014 ohm-cm | |
Surface Resistance | 1e+014 ohm | |
Comparative Tracking Index | 600 V | |
Thermal Properties |
|
CTE, linear 20°C | 80 µm/m-°C | Parallel to flow |
Melting Point | 174 °C | (Dry) |
Deflection Temperature at 0.46 MPa (66 psi) | 143 °C | |
Deflection Temperature at 1.8 MPa (264 psi) | 65 °C | |
Vicat Softening Point | 145 °C | 50°C/hr; 50N |
Flammability, UL94 | HB | 3.1 mm |
Flammability, UL94 | HB | 1.6 mm |
|
Printer friendly version |
|