SABIC Innovative Plastics ULTEM AR9300 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
Physical Properties | Original Value | Comments |
|
Density | 1.49 g/cc | ASTM D 792 |
Linear Mold Shrinkage | 0.002 - 0.004 cm/cm | Flow, 0.125 inch; ASTM D 955 |
Melt Flow | 4.2 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
Tensile Strength @ Break | 22500 psi | Type I, 0.2 in/min; ASTM D 638 |
Elongation at Break | 3 % | Type I, 0.2 in/min; ASTM D 638 |
Tensile Modulus | 1.3e+006 psi | 0.2 in/min; ASTM D 638 |
Flexural Modulus | 1.4e+006 psi | 0.10 in/min, 4" span; ASTM D 790 |
Flexural Yield Strength | 35000 psi | 0.10 in/min, 4" span; ASTM D 790 |
Izod Impact, Notched | 10 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Izod Impact, Notched | 2.2 ft-lb/in | 73F; ASTM D 256 |
Thermal Properties |
|
Deflection Temperature at 1.8 MPa (264 psi) | 414 °F | 0.250 inch, unannealed; ASTM D 648 |
Flammability Test | 0 | Vertical Burn, extinguish time; seconds; FAR 25.853 |
Flammability Test | 0 | Vertical Burn, drip time; seconds; FAR 25.853 |
Flammability Test | 3.5 | Vertical Burn, length; inches; FAR 25.853 |
Flammability Test | 40 | OSU Peak Heat Release Rate (horizontal); KW/m2; FAR 25.853 |
Flammability Test | 5 | OSU 2 minute heat, release rate; KW-Min/m2; FAR 25.853 |
NBS Smoke Density | 0 | Flaming, Ds 1.5 min; ASTM E 662 |
NBS Smoke Density | 5 | Flaming, Dmax; ASTM E 662 |
NBS Smoke Density | 5 | Flaming, Ds 4 min; ASTM E 662 |
Descriptive Properties | |
FAR 25.853 | NATURAL | |
|