SABIC Innovative Plastics ULTEM CRS5011 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Original Value | Comments |
|
| Density | 1.28 g/cc | ASTM D 792 |
| Linear Mold Shrinkage | 0.004 - 0.007 cm/cm | Flow, 0.125 inch; ASTM D 955 |
| Melt Flow | 11 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Yield | 14500 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 60 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 420000 psi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 450000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 20000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Izod Impact, Notched | 1.1 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 39 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Electrical Properties |
|
| Dielectric Constant | 3.2 | 50 Hz; ASTM D 150 |
| Dielectric Strength | 457 V/mil | in oil, 125 mils; ASTM D 149 |
| Dissipation Factor | 0.0021 | 50 Hz; ASTM D 150 |
| Arc Resistance | 120 - 180 sec | Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495 |
| Comparative Tracking Index | 100 - 175 V | (+/- 0.125 inch); PLC Code 4; UL 746A |
| Hot Wire Ignition, HWI | Min 120 sec | (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Amp Arc Ignition, HAI | Min 120 arcs | Surface (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80 mm/min | (+/- 0.125 inch); PLC Code 2; UL 746A |
Thermal Properties |
|
| Deflection Temperature at 1.8 MPa (264 psi) | 400 °F | 0.250 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 160 °C | UL 746B |
| UL RTI, Mechanical with Impact | 155 °C | UL 746B |
| UL RTI, Mechanical without Impact | 160 °C | UL 746B |
| Flammability, UL94 | V-0 | 0.058 in. |
Descriptive Properties | |
| CSA File No. | LS88480 | |
| UL File Number, USA | E121562 | |
|