SABIC Innovative Plastics ULTEM 1285 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Original Value | Comments |
|
| Density | 1.29 g/cc | ASTM D 792 |
| Linear Mold Shrinkage | 0.006 - 0.007 cm/cm | Flow, 0.125 inch; ASTM D 955 |
| Melt Flow | 8.1 g/10 min | 295C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Break | 12000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Strength @ Yield | 16000 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 60 % | Type I, 0.2 in/min; ASTM D 638 |
| Tensile Modulus | 490000 psi | 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 490000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Yield Strength | 24000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Gardner Impact @ 23°C | 360 in-lb | Instrumented Impact Total Energy, 73°F; ASTM D 3763 |
| Izod Impact, Notched | 0.5 ft-lb/in | 73F; ASTM D 256 |
| Izod Impact, Notched | 17.8 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Thermal Properties |
|
| CTE, linear 68°F | 27 µin/in-°F | Flow, -40F to 100F; ASTM E 831 |
| CTE, linear 68°F, Transverse to Flow | 27 µin/in-°F | from -40F to 100F; ASTM E 831 |
| Deflection Temperature at 1.8 MPa (264 psi) | 329 °F | 0.250 inch, unannealed; ASTM D 648 |
| Vicat Softening Point | 358 °F | Rate B; ASTM D 1525 |
|