SABIC Innovative Plastics ULTEM 4001 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
Physical Properties | Original Value | Comments |
|
Density | 1.33 g/cc | ASTM D 792 |
Linear Mold Shrinkage | 0.005 - 0.007 cm/cm | Flow, 0.125 inch; ASTM D 955 |
Melt Flow | 9.5 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
Hardness, Rockwell M | 110 | ASTM D 785 |
Tensile Strength @ Yield | 15000 psi | Type I, 0.2 in/min; ASTM D 638 |
Elongation at Break | 40 % | Type I, 0.2 in/min; ASTM D 638 |
Tensile Modulus | 487000 psi | 0.2 in/min; ASTM D 638 |
Flexural Modulus | 494000 psi | 0.10 in/min, 4" span; ASTM D 790 |
Flexural Yield Strength | 22000 psi | 0.10 in/min, 4" span; ASTM D 790 |
Izod Impact, Unnotched | 10 ft-lb/in | 73F; ASTM D 4812 |
Coefficient of Friction | 0.25 | Vs. Steel, Kinetic; ASTM D 1894 |
K (wear) Factor | 27 x 10-10 in³-min/ft-lb-hr | PV=2000 psi-fpm vs Self; GE Test |
K (wear) Factor | 72 x 10-10 in³-min/ft-lb-hr | PV = 2000 psi-fpm vs Steel; GE Test |
Limiting Pressure Velocity | 55000 psi-ft/min | 100 fpm; GE Test |
Taber Abrasion, mg/1000 Cycles | 2 | CS-17, 1 kg; ASTM D 1044 |
Izod Impact, Notched | 2.2 ft-lb/in | 73F; ASTM D 256 |
Izod Impact, Notched | 24 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Electrical Properties |
|
Arc Resistance | 60 - 120 sec | Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495 |
Comparative Tracking Index | 100 - 175 V | (+/- 0.125 inch); PLC Code 4; UL 746A |
Hot Wire Ignition, HWI | 60 - 120 sec | (+/- 0.125 inch); PLC Code 1; UL 746A |
High Amp Arc Ignition, HAI | Min 120 arcs | Surface (+/- 0.125 inch); PLC Code 0; UL 746A |
High Voltage Arc-Tracking Rate, HVTR | 25.4 - 80 mm/min | (+/- 0.125 inch); PLC Code 2; UL 746A |
Thermal Properties |
|
Deflection Temperature at 1.8 MPa (264 psi) | 392 °F | 0.250 inch, unannealed; ASTM D 648 |
UL RTI, Electrical | 170 °C | UL 746B |
UL RTI, Mechanical with Impact | 170 °C | UL 746B |
UL RTI, Mechanical without Impact | 170 °C | UL 746B |
Flammability, UL94 | V-0 | 0.015 in. |
Flammability, UL94 | 7 | 0.059 in. |
Descriptive Properties | |
UL File Number, USA | E121562 | |
|