SABIC Innovative Plastics ULTEM 4211 Polyetherimide (North America)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
| Physical Properties | Original Value | Comments |
|
| Density | 1.48 g/cc | ASTM D 792 |
| Melt Flow | 10.3 g/10 min | 337C/6.6 kgf; ASTM D 1238 |
Mechanical Properties |
|
| Tensile Strength @ Yield | 18750 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 3 % | Type I, 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 1.03e+006 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Flexural Strength | 28000 psi | 0.10 in/min, 4" span; ASTM D 790 |
| Izod Impact, Notched | 8.2 ft-lb/in | Reverse Notched, 73F; ASTM D 256 |
Thermal Properties |
|
| Deflection Temperature at 1.8 MPa (264 psi) | 414 °F | 0.250 inch, unannealed; ASTM D 648 |
|