SABIC Innovative Plastics VALOX 327 PBT (North America)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line.
| Physical Properties | Original Value | Comments |
|
| Density | 1.29 g/cc | ASTM D 792 |
| Water Absorption | 0.08 % | 24 hours @ 73F; ASTM D 570 |
| Linear Mold Shrinkage | 0.014 - 0.018 cm/cm | Flow, 30-90 mil; ASTM D 955 |
| Linear Mold Shrinkage | 0.017 - 0.023 cm/cm | Flow, 90-180 mil; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.014 - 0.018 cm/cm | 30-90 mil; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.017 - 0.022 cm/cm | 90-180 mil; ASTM D 955 |
Mechanical Properties |
|
| Tensile Strength @ Yield | 7000 psi | Type I, 2.0 in/min; ASTM D 638 |
| Elongation at Break | 200 % | Type I, 2.0 in/min; ASTM D 638 |
| Flexural Modulus | 320000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Yield Strength | 12000 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Notched | 1.5 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | 1e+017 ohm-cm | ASTM D 257 |
| Dielectric Constant | 2.9 | 1 MHz; ASTM D 150 |
| Dielectric Strength | 406 V/mil | in air, 32 mils; ASTM D 149 |
| Dissipation Factor | 0.02 | 1 MHz; ASTM D 150 |
Thermal Properties |
|
| Deflection Temperature at 0.46 MPa (66 psi) | 305 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 130 °F | 0.250 inch, unannealed; ASTM D 648 |
|