SABIC Innovative Plastics VALOX 371 PBT (North America)

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)
 Export data to your CAD/FEA program

Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their North American product line.

Physical PropertiesOriginal ValueComments
Density1.39 g/cc ASTM D 792
Water Absorption0.08 % 24 hours @ 73F; ASTM D 570
Linear Mold Shrinkage0.009 - 0.016 cm/cm Flow, 30-90 mil; ASTM D 955
Linear Mold Shrinkage0.015 - 0.023 cm/cm Flow, 90-180 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.01 - 0.017 cm/cm 30-90 mil; ASTM D 955
Linear Mold Shrinkage, Transverse0.016 - 0.024 cm/cm 90-180 mil; ASTM D 955

Mechanical Properties
Hardness, Rockwell R120 ASTM D 785
Tensile Strength @ Break8500 psi Type I, 2.0 in/min; ASTM D 638
Tensile Strength @ Yield8500 psi Type I, 2.0 in/min; ASTM D 638
Elongation at Break80 % Type I, 2.0 in/min; ASTM D 638
Flexural Modulus380000 psi 0.05 in/min, 2" span; ASTM D 790
Flexural Strength14700 psi 0.05 in/min, 2" span; ASTM D 790
Flexural Yield Strength14700 psi 0.05 in/min, 2" span; ASTM D 790
Izod Impact, Unnotched30 ft-lb/in 73F; ASTM D 4812
Gardner Impact25 ft-lb 73F; ASTM D 3029
Gardner Impact25 ft-lb Modified Gardner, 73F; ASTM D 3029
Izod Impact, Notched0.7 ft-lb/in 73F; ASTM D 256

Electrical Properties
Volume ResistivityMin 1.6e+016 ohm-cm ASTM D 257
Dielectric Constant3.1 100 Hz; ASTM D 150
Dielectric Constant3.1 1 MHz; ASTM D 150
Dielectric Strength468 V/mil in air, 125 mils; ASTM D 149
Dielectric Strength560 V/mil in oil, 62 mils; ASTM D 149
Dissipation Factor0.002 100 Hz; ASTM D 150
Dissipation Factor0.02 1 MHz; ASTM D 150
Arc Resistance60 - 120 sec Tungsten (+/- 0.125 inch); PLC Code 6; ASTM D 495
Comparative Tracking Index175 - 250 V (+/- 0.125 inch); PLC Code 3; UL 746A
Hot Wire Ignition, HWI30 - 60 sec (+/- 0.125 inch); PLC Code 2; UL 746A
High Amp Arc Ignition, HAIMin 120 arcs Surface (+/- 0.125 inch); PLC Code 0; UL 746A
High Voltage Arc-Tracking Rate, HVTRMin 150 mm/min (+/- 0.125 inch); PLC Code 4; UL 746A

Thermal Properties
CTE, linear 68°F44 µin/in-°F Flow, -40F to 100F; ASTM E 831
CTE, linear, 212°F (100°C)73 µin/in-°F Flow, 140F to 280F; ASTM E 831
Deflection Temperature at 0.46 MPa (66 psi)325 °F 0.250 inch, unannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi)160 °F 0.250 inch, unannealed; ASTM D 648
UL RTI, Electrical120 °C UL 746B
UL RTI, Mechanical with Impact120 °C UL 746B
UL RTI, Mechanical without Impact140 °C UL 746B
Flammability, UL94V-0 0.028 in.
Flammability, UL947 0.118 in.

Descriptive Properties
CSA File No.LS88480 
UL File Number, USAE121562 
Printer friendly version Printer friendly version


Instant Quotes for Quick Parts!Upload your 3D CAD model, select process, quantity, material, and instantly receive your unique, binding quote.

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。