SABIC Innovative Plastics VALOX 420 PBT (North America)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their North American product line. MatWeb has a separate entry for the European data sheet.
| Physical Properties | Original Value | Comments |
|
| Density | 1.53 g/cc | ASTM D 792 |
| Water Absorption | 0.06 % | 24 hours @ 73F; ASTM D 570 |
| Linear Mold Shrinkage | 0.003 - 0.005 cm/cm | Flow, 60-125 mil; ASTM D 955 |
| Linear Mold Shrinkage | 0.005 - 0.008 cm/cm | Flow, 125-180 mil; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.004 - 0.006 cm/cm | 60-125 mil; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.006 - 0.009 cm/cm | 125-180 mil; ASTM D 955 |
Mechanical Properties |
|
| Hardness, Rockwell R | 118 | ASTM D 785 |
| Tensile Strength @ Break | 17300 psi | Type I, 0.2 in/min; ASTM D 638 |
| Elongation at Break | 3 % | Type I, 0.2 in/min; ASTM D 638 |
| Flexural Modulus | 1.1e+006 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Flexural Strength | 27500 psi | 0.05 in/min, 2" span; ASTM D 790 |
| Izod Impact, Unnotched | 15 ft-lb/in | 73F; ASTM D 4812 |
| Izod Impact, Notched | 1.6 ft-lb/in | 73F; ASTM D 256 |
Electrical Properties |
|
| Volume Resistivity | Min 3.2e+016 ohm-cm | ASTM D 257 |
| Dielectric Constant | 3.7 | 1 MHz; ASTM D 150 |
| Dielectric Constant | 3.8 | 100 Hz; ASTM D 150 |
| Dielectric Strength | 475 V/mil | in air, 125 mils; ASTM D 149 |
| Dielectric Strength | 630 V/mil | in oil, 62 mils; ASTM D 149 |
| Dissipation Factor | 0.002 | 100 Hz; ASTM D 150 |
| Dissipation Factor | 0.02 | 1 MHz; ASTM D 150 |
| Arc Resistance | 120 - 180 sec | Tungsten (+/- 0.125 inch); PLC Code 5; ASTM D 495 |
| Comparative Tracking Index | Min 600 V | (+/- 0.125 inch); PLC Code 0; UL 746A |
| High Voltage Arc-Tracking Rate, HVTR | 10 - 25.4 mm/min | (+/- 0.125 inch); PLC Code 1; UL 746A |
Thermal Properties |
|
| CTE, linear 68°F | 14 µin/in-°F | Flow, -40F to 100F; ASTM E 831 |
| CTE, linear, 212°F (100°C) | 14 µin/in-°F | Flow, 140F to 280F; ASTM E 831 |
| Deflection Temperature at 0.46 MPa (66 psi) | 420 °F | 0.250 inch, unannealed; ASTM D 648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 405 °F | 0.250 inch, unannealed; ASTM D 648 |
| UL RTI, Electrical | 140 °C | UL 746B |
| UL RTI, Mechanical with Impact | 140 °C | UL 746B |
| UL RTI, Mechanical without Impact | 140 °C | UL 746B |
| Flammability, UL94 | HB | 0.033 in. |
| Oxygen Index | 19 % | ASTM D 2863 |
Descriptive Properties | |
| CSA File No. | LS88480 | |
| UL File Number, USA | E121562 | |
|
Printer friendly version |
|