| Physical Properties | Original Value | Comments |
|
| Density | 1.34 g/cc | ASTM D 792 |
| Density | 1.34 g/cc | ISO 1183 |
| Moisture Absorption at Equilibrium | 0.15 % | (23 C / 50% RH) 1L; ISO 15512 |
| Water Absorption at Saturation | 0.5 % | 23C; ISO 62 |
| Linear Mold Shrinkage | 0.011 - 0.018 cm/cm | Flow; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.009 - 0.018 cm/cm | ASTM D 955 |
| Melt Flow | 8 g/10 min | cm3/10min; Melt Volume Rate, MVR at 250C/5.0 kg; ISO 1133 |
Mechanical Properties |
|
| Hardness, Rockwell R | 117 | ISO 2039/2 |
| Hardness, H358/30 | 111 MPa | ISO 2039/1 |
| Tensile Strength, Yield | 50 MPa | 50 mm/min; ISO 527 |
| Elongation at Break | 30 % | 50 mm/min; ISO 527 |
| Elongation at Yield | 5 % | 50 mm/min; ISO 527 |
| Tensile Modulus | 2.2 GPa | 1 mm/min; ISO 527 |
| Flexural Modulus | 2 GPa | 2 mm/min; ISO 178 |
| Flexural Yield Strength | 80 MPa | 2 mm/min; ISO 178 |
| Izod Impact, Notched (ISO) | 45 kJ/m² | 80*10*4 +23 C; ISO 180/ 1A |
| Izod Impact, Unnotched (ISO) | NB | 80*10*4 +23 C; ISO 180/ 1U |
| Izod Impact, Unnotched Low Temp (ISO) | NB | 80*10*4 -30 C; ISO 180/ 1U |
| Izod Impact, Notched, Low Temp (ISO) | 10 kJ/m² | 80*10*4 -30 C; ISO 180/ 1A |
| Charpy Impact Unnotched | NB | 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
| Charpy Impact, Notched, Low Temp | 2 J/cm² | at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
| Charpy Impact, Unnotched Low Temp | NB | at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
| Charpy Impact, Notched | 1.5 J/cm² | 23 C; ISO 179/2C |
| Charpy Impact, Notched | 4.5 J/cm² | 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
| Taber Abrasion, mg/1000 Cycles | 33 | CS-17, 1 kg; GE Test |
Electrical Properties |
|
| Volume Resistivity | Min 1e+015 ohm-cm | IEC 60093 |
| Surface Resistivity per Square | Min 1e+015 ohm | ROA; IEC 60093 |
| Dielectric Constant | 2.9 | 1 MHz; IEC 60250 |
| Dielectric Constant | 3 | 50 Hz; IEC 60250 |
| Dielectric Strength | 18 kV/mm | in oil, 3.2 mm; IEC 60243-1 |
| Dielectric Strength | 26 kV/mm | in oil, 1.6 mm; IEC 60243-1 |
| Dielectric Strength | 34 kV/mm | in oil, 0.8 mm; IEC 60243-1 |
| Dissipation Factor | 0.002 | 50 Hz; IEC 60250 |
| Dissipation Factor | 0.007 | 1 MHz; IEC 60250 |
| Comparative Tracking Index | 100 V | M; IEC 60112/3rd |
| Comparative Tracking Index | 225 V | IEC 60112/3rd |
Thermal Properties |
|
| CTE, linear 20°C | 100 µm/m-°C | 23C-80C, flow; ISO 11359-2 |
| CTE, linear 20°C Transverse to Flow | 100 µm/m-°C | 23C-80C; ISO 11359-2 |
| Thermal Conductivity | 0.17 W/m-K | ISO 8302 |
| Deflection Temperature at 0.46 MPa (66 psi) | 135 °C | HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be |
| Deflection Temperature at 1.8 MPa (264 psi) | 85 °C | HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae |
| Vicat Softening Point | 145 °C | B/50; ISO 306 |
| Vicat Softening Point | 150 °C | B/120; ISO 306 |
| Vicat Softening Point | 180 °C | A/50; ISO 306 |
| UL RTI, Electrical | 120 °C | UL 746B |
| UL RTI, Mechanical with Impact | 120 °C | UL 746B |
| UL RTI, Mechanical without Impact | 140 °C | UL 746B |
| Flammability, UL94 | V-0 | 0.75 mm |
| Flammability, UL94 | 7 | 94-2 mm |
| Flammability Test | 3.2 | mm; IEC Needle Flame Test, 10 s , passes at; IEC 60695-2-2 |
| Oxygen Index | 30 % | ISO 4589 |
| Glow Wire Test | 960 °C | Passes at 1 mm; IEC 60695-2-1 |
Descriptive Properties |
|
| Ball Pressure Test, 125 C +/- 2 C | PASSES | IEC 60035-1 |
| Needle Flame Test, 3.2 mm, Burn Time s | PASSES | IEC 60695-2-2 |
|
Printer friendly version |