SABIC Innovative Plastics VALOX 7523 PBT (Europe)

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)
 Export data to your CAD/FEA program

Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic

Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.

Material Notes:
Information provided by GE Plastics for their European product line.

Physical PropertiesOriginal ValueComments
Density1.82 g/cc ASTM D 792
Density1.82 g/cc ISO 1183
Water Absorption0.06 % Moisture Absorption, 50% RH, 24 hrs; ASTM D 570
Moisture Absorption at Equilibrium0.09 % (23 C / 50% RH) 1L; ISO 15512
Water Absorption at Saturation0.94 % 23C; ISO 62
Linear Mold Shrinkage0.002 - 0.005 cm/cm Flow; ASTM D 955
Linear Mold Shrinkage, Transverse0.008 - 0.015 cm/cm ASTM D 955
Melt Flow17 g/10 min cm3/10min; Melt Volume Rate, MVR at 250C/5.0 kg; ISO 1133

Mechanical Properties
Hardness, H358/30144 MPa ISO 2039/1
Tensile Strength, Ultimate80 MPa 5 mm/min; ISO 527
Elongation at Break1 % 5 mm/min; ISO 527
Tensile Modulus11 GPa 1 mm/min; ISO 527
Flexural Modulus9.5 GPa 2 mm/min; ISO 178
Flexural Strength130 MPa 2 mm/min; ISO 178
Izod Impact, Notched (ISO)5 kJ/m² 80*10*4 +23 C; ISO 180/ 1A
Izod Impact, Unnotched (ISO)25 kJ/m² 80*10*4 +23 C; ISO 180/ 1U
Izod Impact, Unnotched Low Temp (ISO)12 kJ/m² 80*10*4 -30 C; ISO 180/ 1U
Izod Impact, Notched, Low Temp (ISO)5 kJ/m² 80*10*4 -30 C; ISO 180/ 1A
Charpy Impact Unnotched2 J/cm² 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched, Low Temp0.5 J/cm² at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA
Charpy Impact, Unnotched Low Temp2 J/cm² at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU
Charpy Impact, Notched0.6 J/cm² 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA

Electrical Properties
Volume ResistivityMin 1e+015 ohm-cm IEC 60093
Surface Resistivity per SquareMin 1e+015 ohm ROA; IEC 60093
Dielectric Constant3.2 1 MHz; IEC 60250
Dielectric Constant3.5 50 Hz; IEC 60250
Dielectric Strength18 kV/mm in oil, 3.2 mm; IEC 60243-1
Dielectric Strength23 kV/mm in oil, 1.6 mm; IEC 60243-1
Dissipation Factor0.001 50 Hz; IEC 60250
Dissipation Factor0.014 1 MHz; IEC 60250
Comparative Tracking Index425 V IEC 60112/3rd

Thermal Properties
CTE, linear 20°C25 µm/m-°C 23C-80C, flow; ISO 11359-2
CTE, linear 20°C Transverse to Flow80 µm/m-°C 23C-80C; ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)220 °C HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi)208 °C HDT/Ae, 1.82 MPa Edgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point205 °C B/50; ISO 306
Vicat Softening Point205 °C B/120; ISO 306
Vicat Softening Point215 °C Rate B; ASTM D 1525
Vicat Softening Point215 °C A/50; ISO 306
UL RTI, Electrical130 °C UL 746B
UL RTI, Mechanical with Impact130 °C UL 746B
UL RTI, Mechanical without Impact140 °C UL 746B
Flammability, UL94V-0 0.75 mm
Oxygen Index28 % ISO 4589
Glow Wire Test960 °C Passes at 1.6 mm; IEC 60695-2-1

Descriptive Properties
Ball Pressure Test, 125 C +/- 2 CPASSES IEC 60035-1
Printer friendly version Printer friendly version


Instant Quotes for Quick Parts!Upload your 3D CAD model, select process, quantity, material, and instantly receive your unique, binding quote.

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。