SABIC Innovative Plastics VALOX 830X PBT (Europe)
Subcategory: Polybutylene Terephthalate (PBT); Polyester, TP; Polymer; Thermoplastic
Close Analogs: Saudi Basic Industries Corporation (SABIC) announced on August 31st, 2007, the completion of its purchase of GE Plastics.
Material Notes: Information provided by GE Plastics for their European product line.
| Physical Properties | Original Value | Comments |
|
| Density | 1.54 g/cc | ASTM D 792 |
| Density | 1.54 g/cc | ISO 1183 |
| Moisture Absorption at Equilibrium | 0.08 % | (23 C / 50% RH) 1L; ISO 15512 |
| Water Absorption at Saturation | 0.2 % | 23C; ISO 62 |
| Linear Mold Shrinkage | 0.004 - 0.009 cm/cm | Flow; ASTM D 955 |
| Linear Mold Shrinkage, Transverse | 0.006 - 0.011 cm/cm | ASTM D 955 |
| Melt Flow | 8 g/10 min | cm3/10min; Melt Volume Rate, MVR at 265C/1.2 kg; ISO 1133 |
Mechanical Properties |
|
| Tensile Strength, Ultimate | 105 MPa | 5 mm/min; ISO 527 |
| Elongation at Break | 3 % | 5 mm/min; ISO 527 |
| Tensile Modulus | 8 GPa | 1 mm/min; ISO 527 |
| Flexural Modulus | 7 GPa | 2 mm/min; ISO 178 |
| Flexural Yield Strength | 150 MPa | 2 mm/min; ISO 178 |
| Izod Impact, Notched (ISO) | 5 kJ/m² | 80*10*4 +23 C; ISO 180/ 1A |
| Izod Impact, Unnotched (ISO) | 40 kJ/m² | 80*10*4 +23 C; ISO 180/ 1U |
| Izod Impact, Unnotched Low Temp (ISO) | 30 kJ/m² | 80*10*4 -30 C; ISO 180/ 1U |
| Izod Impact, Notched, Low Temp (ISO) | 5 kJ/m² | 80*10*4 -30 C; ISO 180/ 1A |
| Charpy Impact Unnotched | 3.5 J/cm² | 23C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
| Charpy Impact, Notched, Low Temp | 0.4 J/cm² | at -30C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
| Charpy Impact, Unnotched Low Temp | 2.5 J/cm² | at -30C, Unnotch Edgew 80*10*4 sp=62; ISO 179/1eU |
| Charpy Impact, Notched | 0.5 J/cm² | 23C, V-notch Edgew 80*10*4 sp=62; ISO 179/1eA |
Thermal Properties |
|
| Vicat Softening Point | 175 °C | B/120; ISO 306 |
| Flammability, UL94 | HB | 1.5 mm |
|
Printer friendly version |
|