Physical Properties | Original Value | Comments |
|
Density | 1.28 g/cc | ASTM D792 |
Linear Mold Shrinkage | 0.004 - 0.007 cm/cm | 3.2 mm sample |
Melt Flow | 10.8 g/10 min | 335°C/6.6kg; ASTM D1238 |
Mechanical Properties |
|
Tensile Strength, Ultimate | 100 MPa | ASTM D638 |
Elongation at Break | 70 % | ASTM D638 |
Modulus of Elasticity | 2.9 GPa | ASTM D638 |
Flexural Modulus | 3.1 GPa | 6.4 mm sample; ASTM D790 |
Flexural Yield Strength | 138 MPa | ASTM D790 |
Izod Impact, Notched | 0.3 J/cm | 3.2 mm sample; ASTM D256 |
Thermal Properties |
|
Deflection Temperature at 1.8 MPa (264 psi) | 204 °C | 6.4 mm (0.25 in.) sample; ASTM D648 |
Processing Properties |
|
Processing Temperature | 365 - 387 °C | Suggested injection molding melt temperature |
Mold Temperature | 135 - 162 °C | |
Drying Temperature | 149 °C | |
Dry Time | 4 - 6 hour | 24 hr Max. |
|