PolyOne Stat-Tech™ PI-05CF/000 EM Polyetherimide (PEI)
Subcategory: Polyetherimide; Polymer; Thermoplastic
Material Notes: Stat-Tech™ Electrically Conductive Compounds are specifically engineered to provide anti-static, ESD and RFI/EMI shielding performance for critical electronic equipment applications. These compounds combine the performance of select engineering resins with reinforcing additives such as carbon powder, carbon fiber, nickel-coated carbon fiber and stainless steel fiber, for low-to-high levels of conductivity depending upon application requirements.Description/Features: - PEI (Polyetherimide)
- 5% Carbon Fiber Reinforced
- ESD Protection
- Antistatic
- Static Dissipative
Applications: - EMI?RFI Shielding
- Printer Components
- Enclosures
- Fuel Systems
Processing Method: Injection Molding Information provided by PolyOne Corporation
| Physical Properties | Original Value | Comments |
|
| Specific Gravity | 1.29 g/cc | ASTM D792 |
| Water Absorption | 0.25 % | 24 hr. Immersion, 0.125 in; ASTM D570 |
| Linear Mold Shrinkage | 0.004 - 0.006 cm/cm | ASTM D955 |
Mechanical Properties |
|
| Tensile Strength @ Yield | 18000 psi | Type 1 - Rigids, Yield, 0.2 in/min; ASTM D638 |
| Elongation at Break | 4 - 5 % | Type 1 - Rigids, 0.2 in/min; ASTM D638 |
| Tensile Modulus | 650000 psi | Type 1 - Rigids, 0.2 in/min; ASTM D638 |
| Flexural Modulus | 650000 psi | ASTM D790 |
| Flexural Strength | 28000 psi | ASTM D790 |
| Izod Impact, Notched | 0.9 ft-lb/in | Method A, Injection Molded, 0.250 in bars, 73°F(23°C); ASTM D256 |
Electrical Properties |
|
| Volume Resistivity | 1000 - 100000 ohm-cm | ASTM D257 |
| Surface Resistivity per Square | 1000 - 100000 ohm | ASTM D257 |
Thermal Properties |
|
| Deflection Temperature at 0.46 MPa (66 psi) | 405 °F | Unannealed; ASTM D648 |
| Deflection Temperature at 1.8 MPa (264 psi) | 390 °F | Unannealed; ASTM D648 |
Processing Properties |
|
| Melt Temperature | 670 - 720 °F | Molding |
|
Printer friendly version |
|