PolyOne Geon® 87431 Vinyl Compound - Rigid (RPVC)
Subcategory: Polymer; Thermoplastic; Vinyl
Material Notes:
Description/Features: - NSF Type I
- PPI-2000 psi Rated
- Normal Impact
- Low Flow
Market: - Fittings (Potable Water, DWV, etc.)
Processing Method: PolyOne First ChoiceInformation provided by PolyOne Corporation.
Physical Properties | Original Value | Comments |
|
Specific Gravity | 1.38 g/cc | ASTM D792 |
Linear Mold Shrinkage | 0.002 - 0.005 cm/cm | ASTM D955 |
Mechanical Properties |
|
Hardness, Shore D | 88 | Instantaneous; ASTM D2240 |
Tensile Strength, Yield | 7700 psi | Type 1 - Rigids, 2 in/min; ASTM D638 |
Tensile Modulus | 445000 psi | Type 1 - Rigids, 2 in/min; ASTM D638 |
Flexural Modulus | 480 ksi | ASTM D790 |
Flexural Strength | 13600 psi | ASTM D790 |
Izod Impact, Notched | 0.9 ft-lb/in | Method A, Injection Molded, 0.250 in bars, 73°F (23°C); ASTM D256 |
Izod Impact, Notched | 1 ft-lb/in | Method A, Injection Molded, 0.125 in bars, 73°F (23°C); ASTM D256 |
Thermal Properties |
|
Deflection Temperature at 1.8 MPa (264 psi) | 162 °F | Unannealed, 0.250 in bars; ASTM D648 |
Processing Properties |
|
Melt Temperature | 395 - 400 °F | Molding |
Descriptive Properties | |
Cell Classification D1784 | 12464 | ASTM D1784 |
NSF | Acceptable | Std 14-Plastic Piping Comp. |
NSF | Acceptable | Std 61-Drinking Water Appl. |
Product Form | Pellets/Cubes | |
|