Degussa AG Vestamid® EX9200 Heat & Light Stabilized Nylon 12/PEBA Elastomer
Subcategory: Elastomer, TPE; Nylon; Nylon 12; Polyether Block Amide (PEBA); Polymer; Thermoplastic
Material Notes: Description: Compared to other contending thermoplastic elastomers, PA 12 elastomers are distinguished by the following properties:- They have low density.
- They are highly resistant to chemicals and solvents.
- They are easy to process and color and are easy to overmold.
- They can be decorated easily by means of heat transfer printing.
- They have excellent impact strength at low temperatures.
- Their hardness and flexibility can be varied over a wide range.
- They have high elasticity and good recovery.
- Their mechanical properties are only slightly temperature-dependent.
- They are free of volatile or migrating plasticizers.
Applications: decorative and protective films for sports articles and interior/exterior designs on automobiles Information provided by degussa.
Physical Properties | Original Value | Comments |
|
Density | 1.01 g/cc | ISO 1183 |
Water Absorption at Saturation | 1.5 % | ISO 62 |
Viscosity Test | 190 cm³/g | Viscosity Number; ISO 307 |
Mechanical Properties |
|
Hardness, Shore D | 68 | ISO 868 |
Tensile Strength, Yield | 31 MPa | ISO 527-1, ISO 527-2 |
Elongation at Break | Min 200 % | ISO 527-1, ISO 527-2 |
Elongation at Yield | 19 % | ISO 527-1, ISO 527-2 |
Tensile Modulus | 0.7 GPa | ISO 527-1, ISO 527-2 |
50% Modulus | 0.027 GPa | ISO 527-1, ISO 527-2 |
Charpy Impact Unnotched | NB | 23°C; ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 0.6 J/cm² | -30°C; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | NB | -30°C; ISO 179/1eU |
Charpy Impact, Notched | 3.3 J/cm² | 23°C, Partial Break; ISO 179/1eA |
Electrical Properties |
|
Volume Resistivity | 1e+011 ohm-cm | Spec.; IEC 60093 |
Surface Resistance | 1e+013 ohm | Spec.; IEC 60093 |
Dielectric Constant | 4.6 | 23°C/1 MHz; IEC 60250 |
Dielectric Constant, Low Frequency | 7.4 | 23°C/100 Hz; IEC 60250 |
Dielectric Strength | 30 kV/mm | K20/P50; IEC 60243-1 |
Dissipation Factor | 0.076 | 23°C/1 MHz; IEC 60250 |
Dissipation Factor, Low Frequency | 0.15 | 23°C/100 Hz; IEC 60250 |
Comparative Tracking Index | 600 V | Test Solution A; IEC 60112 |
Thermal Properties |
|
CTE, linear 20°C | 160 µm/m-°C | 23-55°C, Longitudinal; ISO 11359 |
CTE, linear 20°C | 160 µm/m-°C | 23-55°C, Transverse; ISO 11359 |
Deflection Temperature at 0.46 MPa (66 psi) | 100 °C | ISO 75-2 |
Deflection Temperature at 1.8 MPa (264 psi) | 45 °C | ISO 75-1 |
Vicat Softening Point | 130 °C | 50N; ISO 306 |
Vicat Softening Point | 170 °C | 10N; ISO 306 |
Flammability, UL94 | HB | 1.6 mm |
|
Printer friendly version |
|