Degussa AG Vestamid® LX9007 Nylon 12
Subcategory: Nylon; Nylon 12; Polymer; Thermoplastic
Key Words: PA12, EL,22-010
Material Notes: Description: High-viscosity, light-stabilized Applications: Transparent, scratch-resistant, and printable decorative films Information provided by degussa.
Physical Properties | Original Value | Comments |
|
Density | 1.01 g/cc | ISO 1183 |
Moisture Absorption at Equilibrium | 0.7 % | 23°C/50% R.H. (1mm); ISO 62 |
Water Absorption at Saturation | 1.6 % | 1 mm; ISO 62 |
Linear Mold Shrinkage | 0.012 cm/cm | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
Linear Mold Shrinkage, Transverse | 0.014 cm/cm | 127x12.7x3.2 mm (processing cond. acc. To ISO 1874-2) |
Mechanical Properties |
|
Tensile Strength, Yield | 47 MPa | ISO 527-1/2 |
Elongation at Break | Min 50 % | ISO 527-1/2 |
Elongation at Yield | 5 % | ISO 527-1/2 |
Tensile Modulus | 1.4 GPa | ISO 527-1/2 |
Charpy Impact Unnotched | NB | 23°C; ISO 179/1eU |
Charpy Impact, Notched, Low Temp | 0.9 J/cm² | -30°C; ISO 179/1eA |
Charpy Impact, Unnotched Low Temp | NB | -30°C; ISO 179/1eU |
Charpy Impact, Notched | 1.6 J/cm² | 23°C; ISO 179/1eA |
Electrical Properties |
|
Volume Resistivity | 1e+015 ohm-cm | IEC 60093 |
Dielectric Constant | 3 | 23°C/1 MHz; IEC 60250 |
Dielectric Constant, Low Frequency | 3.7 | 23°C/100 Hz; IEC 60250 |
Dielectric Strength | 26 kV/mm | K20/P50; IEC 60243-1 |
Dissipation Factor | 0.026 | 23°C/1 MHz; IEC 60250 |
Dissipation Factor, Low Frequency | 0.045 | 23°C/100 Hz; IEC 60250 |
Comparative Tracking Index | Min 600 V | Test Solution A, 50 drops; IEC 60112 |
Comparative Tracking Index | 600 V | Test Solution A, 100 drops; IEC 60112 |
Thermal Properties |
|
CTE, linear 20°C | 140 µm/m-°C | 23-55°C (45x15x10 mm); ISO 11359 |
Melting Point | 178 °C | Peak Temperature; ISO 3146, ISO 11357 |
Deflection Temperature at 0.46 MPa (66 psi) | 110 °C | ISO 75 |
Deflection Temperature at 1.8 MPa (264 psi) | 50 °C | ISO 75 |
Vicat Softening Point | 140 °C | 50N; ISO 306 |
Vicat Softening Point | 170 °C | 10N; ISO 306 |
Flammability, UL94 | HB | 3.2 mm |
Flammability, UL94 | HB | 1.6 mm |
Descriptive Properties | |
Electrolytic Corrosion | A1 Step | IEC 60426 |
|
Printer friendly version |
|