BASF Elastollan® 1175A10W Wire & Cable Grade Polyurethane Elastomer
Subcategory: Elastomer, TPE; Polymer; Polyurethane, TP; Thermoplastic
Key Words: TPU Rubbers
Material Notes: As with all TPU products this grade must be dried prior to processing. Information provided by BASF Corporation.
Click here to view available vendors for this material.
Physical Properties | Original Value | Comments |
|
Density | 1.14 g/cc | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D792 |
Mechanical Properties |
|
Hardness, Shore A | 75 | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D2240 |
Tensile Strength, Ultimate | 41 MPa | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C; ASTM D412 |
Tensile Strength, Yield | 11 MPa | Tensile stress at 300% elongation; 0.76 mm (0.030 in) extruded sheet; ASTM D-412 |
Tensile Strength, Yield | 4.8 MPa | Tensile stress at 100% elongation.; ASTM D-412 |
Elongation at Break | 685 % | on 0.030 in extruded sheet; ASTM D-412 |
Flexural Modulus | 0.025 GPa | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D790 |
Tear Strength | 27 kN/m | Split tear strength (ASTM D-1938) on 0.76 mm ( 0.030 inch) extruded sheet |
Graves Tear Strength | 57 kN/m | on 0.76 mm ( 0.030 inch) extruded sheet; ASTM D624 |
Taber Abrasion, mg/1000 Cycles | 20 | H-18 wheel; ASTM D-1044; 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C. |
Compression Set | 25 % | 22 hr at 23°C per ASTM D-395; 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C. |
Compression Set, Elevated Temperature | 45 % | 22 hr @ 70°C; ASTM D-395; 0.080 in molded plaque after curing 20 hrs at 100°C. |
Tensile Set | 32 % | at 200% elongation per ASTM D-412 is on 0.030 in extruded sheet. |
Thermal Properties |
|
Vicat Softening Point | 80 °C | 2.0 mm (0.080 in) molded plaque, cured 20 hr at 100°C.; ASTM D1525 |
Glass Temperature | -47 °C | Pellet sample |
Flammability, UL94 | V-2 | Color: NC; 1.59 mm |
Flammability, UL94 | V-2 | Color: NC; 3.14 mm |
Flammability, UL94 | V-0 | Color: NC; 0.9 mm |
|