Cobalt, Co
Subcategory: Metal; Nonferrous Metal; Pure Element
| Component | Wt. % |  | | | Co | 100 | |
|
Click here to view available vendors for this material.
| Physical Properties | Metric | English | Comments |
|
| Density | 8.8 g/cc | 0.318 lb/in³ | |
Mechanical Properties |
|
| Hardness, Brinell | 125 | 125 | |
| Hardness, Vickers | 253 | 253 | |
| Tensile Strength, Yield | 225 MPa | 32600 psi | |
| Modulus of Elasticity | 211 GPa | 30600 ksi | |
| Poisson's Ratio | 0.32 | 0.32 | |
| Shear Modulus | 82.6 GPa | 12000 ksi | |
Electrical Properties |
|
| Electrical Resistivity | 6.24e-006 ohm-cm | 6.24e-006 ohm-cm | |
| Magnetic Permeability | Max 245 | Max 245 | |
| Magnetic Permeability | 68 | 68 | Initial |
| Curie Temperature | 1121 °C | 2050 °F | |
Thermal Properties |
|
| Heat of Fusion | 259.6 J/g | 112 BTU/lb | |
| CTE, linear 20°C | 12.5 µm/m-°C | 6.94 µin/in-°F | over the range 20-100ºC |
| CTE, linear 250°C | 14.2 µm/m-°C | 7.89 µin/in-°F | at 200°C |
| Specific Heat Capacity | 0.44 J/g-°C | 0.105 BTU/lb-°F | |
| Thermal Conductivity | 69.21 W/m-K | 480 BTU-in/hr-ft²-°F | |
| Melting Point | 1493 °C | 2720 °F | |
Optical Properties |
|
| Emissivity (0-1) | 0.13 | 0.13 | 500°C unoxidized, total spectrum |
| Reflection Coefficient, Visible (0-1) | 0.37 | 0.37 | 200 nm |
| Reflection Coefficient, Visible (0-1) | 0.675 | 0.675 | 1060 nm |
Descriptive Properties | |
| CAS Number | 7440-48-4 | |
|
Printer friendly version |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.

|