Aluminum 1199-O
Subcategory: 1000 Series Aluminum; Aluminum Alloy; Metal; Nonferrous Metal
Close Analogs: Composition Notes: The aluminum content for unalloyed aluminum made by a refining process is the difference between 100.00 percent and the sum of all other metallic elements present in amounts of 0.0010 percent of more each, expressed to the third decimal before determining the sum, which is rounded to the second decimal before subtracting. When an element's specified maximum limit is 0.0XX, an observed value or a calculated value greater than 0.0005 but less than 0.0010% is rounded off and shown as " less than 0.001 ". Composition information provided by the Aluminum Association and is not for design.
Key Words: Aluminium 1199-O; Refined Aluminum; Refined Aluminium; Raffinal; Super-purity Aluminum; UNS A91199, AA11990-O
| Component | Wt. % |  | | | Al | Min 99.99 | | | Cu | Max 0.006 | | | Fe | Max 0.006 | | | Ga | Max 0.005 | |
| | Component | Wt. % |  | | | Mg | Max 0.006 | | | Mn | Max 0.002 | | | Other, each | Max 0.002 | | | Si | Max 0.006 | |
| | Component | Wt. % |  | | | Ti | Max 0.002 | | | V | Max 0.005 | | | Zn | Max 0.006 | |
|
Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.
Click here to view available vendors for this material.
| Physical Properties | Metric | English | Comments |
|
| Density | 2.7 g/cc | 0.0975 lb/in³ | AA; Typical |
Mechanical Properties |
|
| Hardness, Brinell | 12 | 12 | 500 kg load with 10 mm ball. Calculated value. |
| Tensile Strength, Ultimate | 45 MPa | 6530 psi | |
| Tensile Strength, Yield | 10 MPa | 1450 psi | |
| Elongation at Break | 50 % | 50 % | In 5 cm; Sample 1.6 mm thick |
| Modulus of Elasticity | 62 GPa | 8990 ksi | In Tension; Compressive Modulus is about 2% higher |
| Poisson's Ratio | 0.33 | 0.33 | |
| Shear Modulus | 25 GPa | 3630 ksi | |
| Shear Strength | 34 MPa | 4930 psi | Calculated value. |
Electrical Properties |
|
| Electrical Resistivity | 2.7e-006 ohm-cm | 2.7e-006 ohm-cm | |
Thermal Properties |
|
| Heat of Fusion | 390 J/g | 168 BTU/lb | |
| CTE, linear 20°C | 23.6 µm/m-°C | 13.1 µin/in-°F | 20-100ºC |
| CTE, linear 250°C | 25.5 µm/m-°C | 14.2 µin/in-°F | Average over the range 20-300ºC |
| Specific Heat Capacity | 0.9 J/g-°C | 0.215 BTU/lb-°F | |
| Thermal Conductivity | 243 W/m-K | 1690 BTU-in/hr-ft²-°F | |
| Melting Point | 660 - 660 °C | 1220 - 1220 °F | |
| Solidus | 660 °C | 1220 °F | |
| Liquidus | 660 °C | 1220 °F | |
Optical Properties |
|
| Reflection Coefficient, Visible (0-1) | 0.87 | 0.87 | |
|
Printer friendly version |
References for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in
order to display the information in a consistant format. Users requiring more precise data for scientific or
engineering calculations can click on the property value to see the original value as well as raw conversions
to equivalent units. We advise that you only use the original value or one of its raw conversions in your
calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use
regarding this information. Click here to
view all the property values for this datasheet as they were originally entered into MatWeb.
|