MatWeb - Material Property Data 用 MatWeb 登广告!    Register Now
越过59,000 以上, 金属、塑料、陶瓷和合成物的数据资料库。
MatWeb - Material Property Data 主页  •  搜寻  •  工具  •  供应商  •  文件夹  •  有关我们  •  常用问题  •  登录   •  English English English 
  搜寻方法:  高级先进 | 材料类型 | 特性 | 构成份  | 商标  | 制造商
    Search

Buehler
Scientific equipment and supplies for use in materials analysis.

Uninhibited Leaded Muntz Metal, UNS C36500

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)
 Export data to your CAD/FEA program

Subcategory: Copper Alloy; Metal; Nonferrous Metal

Key Words: 60/40 brass, CDA 365, CZ137, ISO, CuZn39Pb0.5, CEN CW610N, UNS C36800, UNS C36600, UNS C36700, UNS C36800, uninhibited, arsenical, antimonial, phosphorized leaded muntz metal, low leaded brass

Component   Wt. %
Cu58 - 61 
FeMax 0.15 
OtherMax 0.1 
Pb0.4 - 0.9 
SnMax 0.25 
Zn39.4 

Material Notes:
Fair to excellent corrosion resistance. Excellent machinability. Combines good machinability with excellent hot formability.

Applications: main tube sheets for condensers and heat exchangers, support sheets, baffles.

Commercial forms available flat products. Rod 61.0% Cu minimum.

Physical PropertiesMetricEnglishComments
Density8.41 g/cc0.304 lb/in³ UNS C36500

Mechanical Properties
Hardness, Rockwell F8080 M20 temper
Tensile Strength, Ultimate370 MPa53700 psi M20 temper
Tensile Strength, Yield140 MPa20300 psi M20 temper
Elongation at Break45 %45 % in 50 mm, M20 temper
Modulus of Elasticity105 GPa15200 ksi 
Poisson's Ratio0.350.35 Calculated
Machinability60 %60 % UNS C36000 (free-cutting brass) = 100%
Shear Modulus39 GPa5660 ksi 

Electrical Properties
Electrical Resistivity6.2e-006 ohm-cm6.2e-006 ohm-cm at 20°C (68°F)

Thermal Properties
CTE, linear 250°C20.8 µm/m-°C11.6 µin/in-°F from 20-300°C (68-570°F)
Specific Heat Capacity0.38 J/g-°C0.0908 BTU/lb-°F 
Thermal Conductivity123 W/m-K854 BTU-in/hr-ft²-°F at 20°C (68°F)
Melting Point885 - 900 °C1630 - 1650 °F 
Solidus885 °C1630 °F 
Liquidus900 °C1650 °F 

Processing Properties
Annealing Temperature425 - 600 °C797 - 1110 °F 
Hot-Working Temperature625 - 800 °C1160 - 1470 °F 
Printer friendly version Printer friendly version

References for this datasheet.


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Buehler
Scientific equipment and supplies for use in materials analysis.

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。