RTP Company RTP 1405 N L Polyethersulfone (PES) Glass Fiber 30% - Lubricated - High Viscosity

Return to last searchReturn to last search
Printer friendly version Printer friendly versionAdd to Folder:
Excel Download Download to Excel (requires Excel and Windows)Material suppliers Material suppliers
 Export data to your CAD/FEA program

Subcategory: Polyethersulfone; Polymer; Thermoplastic

Close Analogs:
Data for this product has not been recently verified, please contact RTP Company for more information before specifying this grade.

Material Notes:
Glass Fiber 30% - Lubricated - High Viscosity

Comments:

  • Glass Fiber
  • Lubricated
  • High Viscosity

Unless otherwise specified, all data listed is for natural or black colored materials. Pigments can affect properties.

Information provided by RTP Company.

Click here to view available vendors for this material.

Physical PropertiesMetricEnglishComments
Specific Gravity1.59 g/cc0.0574 lb/in³ ASTM D792
Filler Content30 %30 % 
Water Absorption0.35 %0.35 % 24 hours at 23°C; ASTM D570
Linear Mold Shrinkage0.002 cm/cm0.002 in/in 1/8 inch (3.18 mm) section; ASTM D955
Linear Mold Shrinkage, 6.35 mm section0.002 cm/cm0.002 in/in 1/4 inch (6.35 mm) section; ASTM D955

Mechanical Properties
Hardness, Rockwell R123123 ASTM D785
Tensile Strength, Ultimate148 MPa21500 psi ASTM D638
Elongation at Break2.6 %2.6 % ASTM D638
Modulus of Elasticity9.65 GPa1400 ksi ASTM D638
Flexural Modulus8.96 GPa1300 ksi ASTM D790
Flexural Yield Strength210 MPa30500 psi ASTM D790
Compressive Yield Strength145 MPa21000 psi ASTM D695
Izod Impact, Unnotched7.47 J/cm14 ft-lb/in 1/8 in (3.18 mm) section; ASTM D256
Izod Impact, Notched0.961 J/cm1.8 ft-lb/in 1/8 in (3.18 mm) section; ASTM D256

Electrical Properties
Electrical Resistivity1e+016 ohm-cm1e+016 ohm-cm ASTM D257
Dielectric Constant4.24.2 1 MHz, Dry; ASTM D150
Dielectric Strength14.6 kV/mm370 V/mil S/T; ASTM D149
Dissipation Factor0.0070.007 1 MHz, Dry; ASTM D150
Arc Resistance75 sec75 sec ASTM D495

Thermal Properties
CTE, linear 68°F27 µm/m-°C15 µin/in-°F Flow Direction; ASTM D696
Thermal Conductivity0.317 W/m-K2.2 BTU-in/hr-ft²-°F Through-plane; ASTM C177
Deflection Temperature at 0.46 MPa (66 psi)221 °C430 °F ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)213 °C415 °F ASTM D648
Flammability, UL94V-0V-0 (V-0) at 1/16 in (1.59 mm); Per testing by RTP Company; ASTM D3801

Processing Properties
Processing Temperature343 - 366 °C650 - 690 °F 
Mold Temperature135 - 177 °C275 - 350 °F 
Injection Pressure68.9 - 103 MPa10000 - 15000 psi 

Descriptive Properties
ColorNatural/Black 
Printer friendly version Printer friendly version


Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistant format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's disclaimer and terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Specialty Compounds RTP Company

<meta http-equiv=Content-Type content="text/html; charset=UTF-8">
请读关于材料数据的使用许可协议和我们的隐私权。询问或评论有关 MatWeb? 请与webmaster@matweb.com 联系。我们感谢您对 MatWeb的参与。

本站点由 Automation Creations, Inc. 设计和维护。这个网站的内容, MatWeb 的商标,与 "MatWeb" 由 Automation Creations, Inc.版权1996-2006拥有 。 MatWeb 意欲为个人使用 , 非商业用途。这个站点的内容、结果和技术数据,未经由 Automation Creations, Inc. 允许, 不可以被电子,摄影或实质上地再生产或自动化创作。